Investigation On Microstructural and Mechanical Properties of B C-Aluminum Matrix Composites Prepared by Microwave Sintering
Investigation On Microstructural and Mechanical Properties of B C-Aluminum Matrix Composites Prepared by Microwave Sintering
Investigation On Microstructural and Mechanical Properties of B C-Aluminum Matrix Composites Prepared by Microwave Sintering
of Pages 5
ARTICLE IN PRESS
j m a t e r r e s t e c h n o l . 2 0 1 5;x x x(x x):xxx–xxx
www.jmrt.com.br
Original Article
a r t i c l e i n f o a b s t r a c t
Article history: B4 C reinforced aluminum composites were fabricated by microwave heating of the mixture
Received 31 August 2014 of B4 C (10, 15 and 20 wt%) and aluminum powders at 650, 750, 850 and 950 ◦ C. The effect of
Accepted 10 February 2015 different amounts of B4 C on the microstructure and mechanical properties of aluminum
Available online xxx matrix was examined. The maximum bending (238 ± 10 MPa) and compressive strength
(330 ± 10 MPa) values were measured for composites sintered at 950 and 750 ◦ C, respectively.
Keywords: The maximum hardness (112 Vickers) was measured for Al–20 wt% B4 C composite sintered
Aluminum at 850 ◦ C. XRD investigations showed the decomposition of boron carbide and also the for-
Boron carbide mation of Al3 BC by heating the composites at 850 ◦ C. SEM micrographs showed uniform
Microwave sintering distribution of reinforcement particles in Al matrix.
Metal matrix composite © 2015 Brazilian Metallurgical, Materials and Mining Association. Published by Elsevier
Editora Ltda. All rights reserved.
∗
Corresponding author.
E-mail: [email protected] (M. Alizadeh).
http://dx.doi.org/10.1016/j.jmrt.2015.02.005
2238-7854/© 2015 Brazilian Metallurgical, Materials and Mining Association. Published by Elsevier Editora Ltda. All rights reserved.
Please cite this article in press as: Ghasali E, et al. Investigation on microstructural and mechanical properties of B4 C–aluminum matrix
composites prepared by microwave sintering. J Mater Res Technol. 2015. http://dx.doi.org/10.1016/j.jmrt.2015.02.005
JMRTEC-153; No. of Pages 5
ARTICLE IN PRESS
2 j m a t e r r e s t e c h n o l . 2 0 1 5;x x x(x x):xxx–xxx
2.45
Al-10wt%B4C
2.4
Al-10wt%B4C-1wt%Co
Table 1 – Different compositions of composite samples. Al-15wt%B4C-1.5wt%Co
2.35 Al-20wt%B4C-2wt%Co
Composite Al (wt%) B4 C (wt%) Co (wt%)
A 90 10 0 2.3
600 650 700 750 800 850 900 950 1000
B 89 10 1
C 83.5 15 1.5 Temperature°C
D 78 20 2
Fig. 2 – Density versus sintering temperature.
Please cite this article in press as: Ghasali E, et al. Investigation on microstructural and mechanical properties of B4 C–aluminum matrix
composites prepared by microwave sintering. J Mater Res Technol. 2015. http://dx.doi.org/10.1016/j.jmrt.2015.02.005
JMRTEC-153; No. of Pages 5
ARTICLE IN PRESS
j m a t e r r e s t e c h n o l . 2 0 1 5;x x x(x x):xxx–xxx 3
Fig. 3 – Backscattered images of B and C composites sintered at 850 ◦ C: (a) Al–10 wt% B4 C–1 wt% Co and (b) Al–15 wt%
B4 C–1.5 wt% Co.
Fig. 4 – Backscattered images of A and B composites sintered at 750 ◦ C: (a) Al–10 wt% B4 C and (b) Al–10 wt% B4 C–1 wt% Co.
Please cite this article in press as: Ghasali E, et al. Investigation on microstructural and mechanical properties of B4 C–aluminum matrix
composites prepared by microwave sintering. J Mater Res Technol. 2015. http://dx.doi.org/10.1016/j.jmrt.2015.02.005
JMRTEC-153; No. of Pages 5
ARTICLE IN PRESS
4 j m a t e r r e s t e c h n o l . 2 0 1 5;x x x(x x):xxx–xxx
250 120
110
Bending strength(MPa)
200
100
150
90
hardness
100
Al-10wt% B4C
80
Al-10wt% B4C-1wt% Co
50 Al-15 wt%B4C-1.5 wt%Co
70
Al-20wt%B4C-2 wt%Co
0 Al-10 wt%B4C
600 650 700 750 800 850 900 950 1000 60
Al-10 wt%B4C-1 wt%Co
Temperature°C
50 Al-15 wt%B4C-1.5 wt%Co
Fig. 6 – A plot showing variation in bending strength of Al-20 wt%B4C-2 wt%Co
40
composites with sintering temperature.
600 650 700 750 800 850 900 950 1000
Temperature°C
The bending strength of B4 C–Al composites fabricated in the Fig. 8 – the effect of sintering temperature on
present work was found to be in the range of 123–238 MPa microhardness on sintered samples.
for B4 C weight percent fractions in the range of 10–20%,
respectively. Fig. 6 illustrates the bending strength changes
of composites versus sintering temperature. As it is clear in The performed studies on the composites fabricated by
Fig. 6, composites have the lowest bending strength among microwave sintering revealed a narrow grain size with uniform
others and Co additive might promote the adhesion of Al to distribution of the reinforcements, and well-bonded inter-
B4 C particles as observed in SEM micrographs (Fig. 4). faces. This may be correlated with the advantage of microwave
The C composites sintered at 650 and 750 ◦ C have higher sintering, which have been proved to produce the composites
bending strength; however, with the raising temperature with small grain size, homogeneous distribution of reinforce-
bending strength of B composites increases (Fig. 6). The inter- ments and proper interfacial characteristic [29,30].
facial reaction and formation of Al3 BC and also more cohesion
between Al matrix and reinforcement as a result of higher 3.6. Microhardness
sintering temperature which causes higher atomic diffusion
could be the possible reason for the above mentioned. It is For all tested samples, the average microhardness of the
obvious that many parameters including interfacial reaction, microwave sintered composites was higher than the cor-
porosity, microcracks, grains size, etc. affect on mechanical responding value for the reference 6061 Al alloy and the
properties of composite; so the evaluation of each individual hardness increased with the increasing amount of B4 C. This
parameter regardless of the impact of others is unreasonable. can be explained by the law of mixtures in the following equa-
tion [19]:
3.5. Compressive strength
Hc = Hm Fm + Hr Fr
The compressive strength results as a function of sintering where Hc , Hm , and Hr are the hardness of the composite,
temperature (Fig. 7) show that an increase in the amount of matrix and reinforcement, respectively, fm and fr are the frac-
B4 C and sintering temperature lead to an increase in the com- tion of matrix and reinforcement, respectively (Fig. 8).
pressive strength. As it was discussed in the bending strength The microhardness increased with increasing reinforce-
section, the smaller grain size will lead to more grain bound- ment, since B4 C is inherently harder than Al matrix and
aries, which can act as strong obstacles to the dislocation the fairly well distribution of the reinforcements improves
motion, leading to the increase of compressive strength. the ability of the soft matrix to resist deformation. Sintering
temperature is another parameter, which influences on the
350 microhardness of the composite. In the Al/B4 C composites,
with raising sintering temperature to 850 ◦ C the microhard-
Compressive strength (MPa)
330
310
ness increased due to decrease in porosity and enhancement
290
of interfacial bonding. At sintering temperature of 950 ◦ C, the
270
250
microhardness of composites decreased probably due to the
Al-10%B4C
230 formation of Al3 BC and the grain coarsening with increasing
210 Al-10%B4C-1%Co sintering temperature.
190 Al-15%B4C-1.5%Co
170 Al-20%B4C-2%Co
150 4. Conclusions
600 650 700 750 800 850 900 950 1000
Temprature°C
Microwave sintering was used successfully to produce Al/B4 C
Fig. 7 – The effect of sintering temperature on compression metal matrix composite. At sintering temperature of 850 ◦ C
strength. and more, the interfacial reaction between Al and B4 C causes
Please cite this article in press as: Ghasali E, et al. Investigation on microstructural and mechanical properties of B4 C–aluminum matrix
composites prepared by microwave sintering. J Mater Res Technol. 2015. http://dx.doi.org/10.1016/j.jmrt.2015.02.005
JMRTEC-153; No. of Pages 5
ARTICLE IN PRESS
j m a t e r r e s t e c h n o l . 2 0 1 5;x x x(x x):xxx–xxx 5
the formation of Al3 BC. 1 wt% cobalt could improve the [13] Halverson DC, Pyzik JA, Aksay IA, Snowden WE. J Am Ceram
microstructural and mechanical properties of the compos- Soc 1989;72:775.
ites. In all composites, the microhardness and compressive [14] Viala JC, Bouix J, Gonzalez G, Esnouf C. Chemical reactivity of
aluminium with boron carbide. J Mater Sci 1997;32:
strength values increased with increasing the weight fraction
4559–73.
of B4 C. Microwave heating could produce Al/B4 C composites [15] Sutton WR. Microwave processing of ceramic materials. Am
along with saving energy and time. Ceram Soc Bull 1989;68(2):376–86.
[16] Clark DE, Folz D, Folgar C, Mahmoud M. Microwave solutions
for ceramic engineering. Westerville, OH, USA: ACerS Pub.;
Conflicts of interest 2005. p. 22–7.
[17] Janney MA, Calhoun CL, Kimrey HD. Microwave sintering of
The authors declare no conflicts of interest. solid oxide fuel cell materials. I. Zirconia–8 mol% yttria. J Am
Ceram Soc 1992;75(2):41–6.
references [18] Goldstein A, Travitzky N, Singurindi A, Kravchik M. Direct
MW sintering of yttria stabilized zirconia at 2.45 GHz. J Eur
Ceram Soc 1999;19(12):2067–74.
[19] Roy R, Agrawal D, Cheng J, Mathis M. Microwave processing:
[1] Ibrahim IA, Mohamed FA, Lavernia EJ. Particulate reinforced triumph of applications-driven science in WC-composites
metal matrix composites – a review. J Mater Sci and ferroic titanates. Ceram Trans 1997;80:3–26.
1991;26:1137–56. [20] Binner JGP, Vaidhyanathan B. Microwave sintering of
[2] Clyne TW, Withers PJ. An introduction to metal matrix ceramics: what does it offer? Key Eng Mater
composites. Cambridge: Cambridge University Press; 1993. 2004;264–268:725–30.
[3] Lloyd DJ. Particle reinforced aluminum and magnesium [21] Goldstein A, Ruginets R, Geffen Y. Microwave sintering of
matrix composites. Int Mater Rev 1994;1:1–39. amorphous silica powders. J Mater Sci Lett 1997;16(4):310–2.
[4] Salvador MD, Amigo V, Martınez N, Busquets D. [22] Ruginets R, Fischer R. Microwave sintering of boron carbide
Microstructure and mechanical behaviour of Al–Si–Mg alloys composites. Bull Am Ceram Soc 1995;74(1):56–8.
reinforced with Ti–Al intermetallics. J Mater Process Technol [23] Viala JC, Bouix J. J Mater Sci 1997;32:4559.
2003;143–144:605–11. [24] Oh S-Y, Cornie JA, Russel KC. Wetting of ceramic particulates
[5] Busquets-Mataix D, Martınez N, Salvador MD, Amigo V. with liquid aluminium alloys. Part I. Experimental
Mechanical and tribological properties of Ti3 Al reinforced techniques. Metall Trans A 1989;20:527–32.
aluminum matrix composites. Adv Compos Lett [25] Oh S-Y, Cornie JA, Russel KC. Wetting of ceramic particulates
2004;13:17–25. with liquid aluminium alloys. Part II. Study of wettability.
[6] Thévenot F. J Eur Ceram Soc 1990;6:205. Metall Trans A 1989;20:533–41.
[7] Chen M, McCauley JW, Hemker KJ. Science 2003;299:1563–6. [26] Marchi CS, Kouzeli M, Miserez A, Moser B, Rossell A, Weber L,
[8] Pyzik JA, Aksay IA. Multipurpose boron carbide–aluminum et al. In: Sang J, Yin R, editors. Proceedings of the advanced
composite and its manufacture via the control of the materials conference (session 3), ICETS-2000 ISAM. Beijing:
microstructure. U.S. Patent No.: 4,702,770 (1987). New World Press; 2000. p. 74–82.
[9] Pyzik JA, Nilsson RT. B4 C–Al cermets and method for making [27] Taya M, Arsenault RJ. Scr Metall 1987;21:349–54.
same. U.S. Patent No.: 5,039,633 (1991). [28] Tham LM, Gupta M, Cheng L. Effect of limited matrix
[10] Halverson DC, Landingham RL. Infiltration processing of reinforcement interfacial reaction on enhancing the
boron carbide, boron, and boride-reactive metal cermets. mechanical properties of aluminium–silicon carbide
U.S. Patent No.: 4,718,941 (1988). composite. Acta Mater 2001;49:3243–53.
[11] Gazza GE. Ceramic-metal systems by infiltration. U.S. Patent [29] Clark DE, Folz DC, West JK. Processing materials with
No.: 3,864,154 (1975). microwave energy. Mater Sci Eng A 2000;287:153–8.
[12] Pyzik JA, Deshmukh UV, Dummead SD, Allen TL, Rossow HE. [30] Clark DE, Sutton WH. Microwave processing of materials.
Light weight boron carbide–aluminum cermets. U.S. Patent Annu Rev Mater Sci 1996;26:299–331.
No.: 5,521,016 (1996).
Please cite this article in press as: Ghasali E, et al. Investigation on microstructural and mechanical properties of B4 C–aluminum matrix
composites prepared by microwave sintering. J Mater Res Technol. 2015. http://dx.doi.org/10.1016/j.jmrt.2015.02.005