Defects in Concrete Monday, 18 November 2019: Title: Date
Defects in Concrete Monday, 18 November 2019: Title: Date
Defects in Concrete
Causes
• Deterioration of concrete structure can be
attributed to many causes. Some of them are:-
– Design deficiencies
– Construction defects
- Material –ingredients selection and compatibility
mixture proportioning.
- poor workmanship, practices.
– Environment –exposure change
– Fire, earthquake etc.
Defects in Concrete
Cracks
• Cracking can be the result of one or a combination of factors
such as
– drying shrinkage,
– thermal contraction,
– restraint (external or internal) to shortening,
– sub-grade settlement,
– applied loads.
• Cracking can not be prevented but it can be significantly
reduced or controlled when the causes are taken into
account and preventative steps are taken
Defects in Concrete
Cracks - continued
• A major problem associated with cracking is layman's perception.
• Cracks can be unsightly but many consumers feel that if a crack
develops in their wall or floor that the product has failed.
• In the case of a wall, if a crack is not structural, if it is not too wide
and there is no water leakage, then there is no cause for concern.
• The acceptability of a crack depends on who you ask.
• It is in our best interest that we educate our customers that the
concrete will crack and when they should become concerned.
Defects in Concrete
Construction Defects
• Material related
– Reactive aggregate
• -Sulphate reactive
• -Alkali reactive aggregate – silica-carbonate
– Corroded steel
– Defective cement
– Unsuitable water
• Inadequate mixture proportioning
– Cement type and content
– w/c control- excess water and extra water-bleeding
– Improper workability
– Improper aggregate grading
– Admixture choice and dosage
Defects in Concrete
Construction Defects
• Workmanship and practices
– Improper alignment of formwork
– Movement of formwork
– Improper reinforcement placement
– Improper consolidation
-honeycombing – inadequate vibration
-segregation –over vibration
– Cold joints- delay in placement
– Improper , inadequate curing
– Premature removal of shuttering and shoring.
Defects in Concrete
Poor formwork
Defects in Concrete
Movement of formwork
Defects in Concrete
Segregation
Defects in Concrete
Stiff concrete
Defects in Concrete
Congested Reinforcement
Defects in Concrete
Plastic settlement
Defects in Concrete
Plastic Settlement
Original
level
Shear
cracks
Void under
steel
Defects in Concrete
Plastic settlement
Defects in Concrete
Plastic Shrinkage
Defects in Concrete
Plastic shrinkage
Defects in Concrete
Workability - slump
Defects in Concrete
Poor vibration
Defects in Concrete
Insufficient cover
Defects in Concrete
Formwork removal
Defects in Concrete
Crazing
• Crazing cracks are very fine and barely visible except when the concrete is
drying after the surface has been wet. The cracks encompass small
concrete areas less than 50 mm (2 in.) in dimension, forming a chicken-
wire pattern.
• The term “map cracking” is often used to refer to cracks that are similar
to crazing cracks only more visible and surrounding larger areas of
concrete.
• Although crazing cracks may be unsightly and can collect dirt, crazing is
not structurally serious and does not ordinarily indicate the start of future
deterioration.
• To prevent crazing, curing procedures should begin early, within minutes
after final finishing when weather conditions warrant.
• When the ambient temperature is high, some method of curing with
water should be used, since this will stop rapid drying and lower the
surface temperature.
• The concrete should be protected against rapid changes in temperature
and moisture wherever feasible.
Defects in Concrete
Crazing
Defects in Concrete
Surface blisters
Defects in Concrete
Causes of blisters
• An excess amount of entrapped air held within the concrete by a high
percentage of fine material ( passing 600 μm, 300 μm, and 150 μm)
• Insufficient vibration during compaction that does not adequately
release entrapped air
• Finishing when the concrete is still spongy. Tools used to compact or
finish the surface will tend to force the entrapped air toward the
surface. Blisters may not appear after the first finishing pass. However,
as the work progresses (during the second or third pass), the front
edge of the trowel blade is lifted to increase the surface density, and
air under the surface skin is forced ahead of the blade until enough is
concentrated(usually near a piece of large aggregate) to form blisters.
Defects in Concrete
How to prevent blistering in concrete
• Do not use concrete with a high slump, excessively high
air content, or excess fines
• Avoid overworking the concrete.
• Do not attempt to seal (finish) the surface too soon.
• Use proper finishing techniques and proper timing during
and between finishing operations.
• Flat floating and flat troweling are often recommended.
• Hand floating should be started when a person standing
on a slab makes a 5-mm (1/4-in.) imprint
Defects in Concrete
De-lamination
Defects in Concrete
De-lamination
• De-laminations are similar to blisters in that delaminated
areas of surface mortar result from bleed water and bleed
air being trapped below the prematurely closed
(densified) mortar surface.
• The primary cause is finishing the surface before bleeding
has occurred.
• De-laminations are also more likely to occur when factors
that extend the bleeding time of concrete (e.g. cold
substrate) are combined with factors that accelerate
surface setting (e.g. high ambient air temperature).
Defects in Concrete
De-lamination
Defects in Concrete
Dusting
Defects in Concrete
Causes of dusting
• Floating and troweling concrete with bleed water on it mixes the
excess water back into the surface, further weakening the concrete’s
strength and wear resistance and giving rise to dusting.
• Dusting may also be caused by
– water applied during finishing,
– exposure to rainfall during finishing,
– spreading dry cement over the surface to accelerate finishing
– low cement content
– too wet a mix
– lack of proper curing (especially allowing rapid drying of the
surface
– dirty aggregate.
Defects in Concrete
Dusting
Defects in Concrete
Joints
• The use of joints is an effective method of
preventing the formation of unsightly cracking.
• If a sizeable length or expanse of concrete, such
as walls, slabs, or pavements, is not provided
with adequate joints to accommodate shrinkage,
the concrete will make its own joints by cracking.
Defects in Concrete
Construction joints – ACI 302.1
• For unreinforced, plain concrete slabs, joint spacing of 24 to 36
times the slab thickness, up to a maximum spacing of 18 ft (5.5
m), have produced acceptable results. Some random cracking
should be expected.
• Joint spacing in nominally reinforced slabs (approximately0.2%
steel placed within 2 in. - 50 mm) of the top of the slab) can be
increased somewhat beyond that recommended for
unreinforced, plain concrete slabs, but the incidence of random
cracking and curling will increase. Reinforcement will not
prevent cracking. If the reinforcement is properly sized and
located, cracks that do occur should remain tightly closed
Defects in Concrete
Joints
Defects in Concrete
Poor construction joint
Defects in Concrete
Good construction joint
Defects in Concrete
Drying shrinkage
• Cracks that occur after hardening usually are the result of drying
shrinkage.
• Hardened concrete will shrink about 1/16 in. in 10 ft of length The
major factors controlling ultimate drying shrinkage of concrete include
relative humidity, aggregate type and content (or paste content), water
content, and w/cm
• The major factor influencing the drying shrinkage properties of
concrete is the total water content of the concrete. As the water
content increases, the amount of shrinkage increases proportionally.
• Large increases in sand content and significant reductions in the size of
the coarse aggregate increase shrinkage, as total water is increased
and smaller size coarse aggregates provide less internal restraint to
shrinkage.
• Within the range of practical concrete mixes 5- to 8-bag mixes cement
content – increases in cement content have little to no effect on
shrinkage as long as the water content is not increased significantly.
Defects in Concrete
Drying shrinkage cracks
Defects in Concrete
General guidelines to reduce- avoid
cracks
• Use proper sub-grade preparation, including uniform support
and proper sub-base material at adequate moisture content.
• Minimize the mix water content by maximizing the size and
amount of coarse aggregate and use low-shrinkage
aggregate.
• Use the lowest amount of mix water required for workability.
• Avoid using excessive amounts of cementitious materials.
• Do not permit overly wet consistencies.
• Prevent rapid loss of surface moisture while the concrete is
still plastic through use of spray-applied finishing aids or
plastic sheets to avoid plastic-shrinkage cracks.
• Provide contraction joints at reasonable intervals, 30 times
the slab thickness.
Defects in Concrete
General guidelines to reduce- avoid
cracks
• Provide isolation joints to prevent restraint from adjoining
elements of a structure.
• Properly place, consolidate, finish, and cure the concrete.
• Consider using synthetic fibers to help control plastic
shrinkage cracks.
Defects in Concrete
Corrosion
Defects in Concrete
Corrosion
Defects in Concrete
Impressed Current Cathodic Protection
Defects in Concrete
Cathodic Protection using sacrificial anode
or Galvanic Protection ( GP)
• Cathodic protection using sacrificial anodes is commonly being
used now a days for protecting reinforced concrete.
• This operates on a similar principal of Cathodic protection, except
that the sacrificial anode, composed of a more reactive metal than
steel (usually zinc), corrodes preferentially to the steel as a result of
a difference in potential between the two metals, thus providing th
necessary current required to maintain the reinforcing steel in
cathodic state.
• Various configurations of the galvanic zinc have been successfully
used to provide cathodic protection in the tidal zone of steel
reinforced concrete structures.
• This simple system is an alternative for their low installation and
maintenance costs, simplicity and by their reliable, self regulating
performance.
Defects in Concrete
Conditions for Alkali Aggregate Reaction-AAR
Defects in Concrete
Alkali-silica reaction (ASR)
• ASR is of more concern because aggregates containing reactive
silica materials are more common.
• In ASR, aggregates containing certain forms of silica will react with
alkali hydroxide in concrete to form a gel that swells as it adsorbs
water from the surrounding cement paste or the environment.
• These gels can swell and induce enough expansive pressure to
damage concrete
Defects in Concrete
ASR
Defects in Concrete
Alkali-carbonate reactions (ACR)
Defects in Concrete