WELDING PROCEDURE WPS No.

: 80-53M
SPECIFICATION (WPS) Ref.: Sour service:

Date: 06.12.23 Rev: 0

Prod. by: Aker Solutions AS Client: Aker BP Ref. stand: EN ISO 15609-1
Project: Hugin A Location: Ref. spec.: NORSOK M-101 Exam. body:
Ref. WPQR: 80-022/80-023 80-051/80-052 80-053/80-054 80-018 / 80-081

Welding process 136


Shielding gas type 1 M21 (Ar+18-22%CO2) 2 3
Weaving (yes/no) Yes max: 20 mm max: mm max: mm

Purging gas type n/a l/min

Welding positions PA, Pb PC, PD PE,PF


Joint type BW, T-BW, FW
Joint preparation Grinding / Sliping
Cleaning before welding Wire brush / stålbørste
Cleaning after welding
Backing n/a
Single/Double bs
Back gouging Arc air / kolstift
Flux designation n/a
Flux handling n/a
Tungsten electrode n/a mm

Torch angle n/a o

Stand off distance 15-20 mm

Nozzle diameter(s) 14-19 mm mm

Tack welding proc. FC-50100-W31-000-EN Rev:


Identification of parent metal I: CE max: 0,43 C max: 0,08 PCM max: 0,19 II: CE max: 0,43 C max: 0,08 PCM max: 0,19

Part Name/Grade Standard Group Delivery cond. Thickness range Diameter


[mm] [mm]

I 500 / Lower grades 500 / Lavere grader 2+1 TMCP 7,50 - 70,00 100 - 9999
II 500 / Lower grades 500 / Lavere grader 2+1 TMCP 7,50 - 70,00 100 - 9999

Identification of filler metal


Index Trade name Classification Group Filler handling
1 NSSW SF-50A AWS A5.36 E91T9-M21A4-K2-H4 FM1 FC-50100-W31-000-EN
2

Welding Parameters Equipment: n/a


Pass Index Dia. Welding Wire feed Current Voltage Current / Welding speed Run Out Length Gas Heat input
no. process speed Polarity
[mm] [m/min] [A] [V] [mm/min] [mm] [l/min] [kJ/mm]
PF - - - - -
1-n 1 1,20 136 6 - 8 180 - 250 20,0 - 25,0 DC+ 190 - 250 1,0 - 2,0
PC - - - - -
1-n 1,20 136 7 - 10 210 - 280 21,0 - 26,0 DC+ 300 - 500 0,5 - 1,5
- - - - -

- - - - -

- - - - -

- - - - -

- - - - -

Heat treatment Method: Heat.torch/Varmebend

Preheat min: 20 °C Interpass temp. max: 250 °C Heat treatment proc.: n/a Temp. control: Temperature crayon

PWHT min: °C max: °C Soaking: min/mm min Heating rate: °C/h Cooling rate: °C/h

Remarks: Heat treatment Method: Electric for thicknesses above 50 mm. Additional info enclosed (Yes/No):
Root opening / Rotåpning: 0-6 mm. Date/Signature:
Root face / Rotkantmål: 0-4 mm. 06.12.23 FRB
Groove angle / Fugevinkel: 35-65°.
Frode Bunes
Approved:
06.12.23 FRB
Frode Bunes
Index no. 309995 Page 1 of 2 Produced by WeldEye®
WP no.:

Welding Parameters 80-53M

Sheet 1 of 1

Pass Index Dia. Welding Wire feed Current Voltage Current / Welding speed Run Out Length Gas Heat input
no. process speed Polarity
[mm] [m/min] [A] [V] [mm/min] [mm] [l/min] [kJ/mm]

- - - - -