1 STICK ELECTRODES
TYPE EN -ISO and ASME -AWS MECHANICAL
PROPERTIES
ANALYSIS APPLICATION
180 HB
CEWELD 9606-1: FM5 T ~ 550 MPa C < 0,04 4332-R is suitable for joining heat resistant CrNi-steels of the same kind and also
4332 R Sect IX QW-432: F-No. 4 Y > 400 MPa Mn 0,5 - 2,5 joining dissimilar metals such as steel to stainless steel. Cladding on low alloyed steels
3581-A: E > 30% Cr 22 - 23 in case a 18/8 CrNi layer is required in the first layer. Scale resistant up to 1050 °C.
E 23 12 LR 32 I > 47J (20 °C) Ni 11 - 14 W.no: 1.4541, 1.4550, 1.4710, 1.4712, 1.4727, 1.4729, 1.4740, 1.4742, 1.4780, 1.4825,
A 5.4: Si < 1,2 1.4826, 1.4828, 1.4878
E 309L-17
CEWELD 9606-1: FM5 T ~ 550 MPa C < 0,04 4332-Ti is a rutile basic electrode for joining heat resistant CrNi-steels of the same
4332 Ti Sect IX QW-432: F-No. 1 Y > 400 MPa Mn 0,5 - 2,5 kind and also joining dissimilar metals such as steel to stainless steel. Cladding on low
3581-A: E > 30% Cr 22 - 23 alloyed steels in case a 18/8 CrNi layer is required in the first layer. Scale resistant up
E 23 12 LR 32 I > 55J (20 °C) Ni 11 - 14 to 1050 °C.
A 5.4: Si < 1,2 W.no: 1.4541, 1.4550, 1.4710, 1.4712, 1.4727, 1.4729, 1.4740, 1.4742, 1.4780, 1.4825,
E 309L-26 1.4826, 1.4828, 1.4878
CEWELD 9606-1: FM5 T ~ 650 MPa C < 0,12 4829-MoTi is suitable for joining heat resistant CrNi(Mo)-steels of the same kind and
4829 MoTi Sect IX QW-432: F-No. 1 Y > 480 MPa Mn 0,5 - 2,5 also joining dissimilar alloys such as steel to stainless steel. Cladding on low alloyed
3581-A: E > 25% Cr 23 - 25 steels in case a 18/8/2 CrNiMo layer is required in the first layer.
E 23 12 2 LR 32 I > 32J (-20 °C) Ni 13 - 14 W.no: 1.4401, 1.4404, 1.4406, 1.4410, 1.4437, 1.4571, 1.4580
A 5.4: Mo 2,0 - 3,0
E 309Mo-26
CEWELD 9606-1: FM5 T ~ 600 MPa C 0,06 - 0,2 4842-Ti is a rutile/basic electrode for welding heat-resistant austenitic steels of the 25%
4842 Ti Sect IX QW-432: F-No. 4 Y > 410 MPa Mn 1,0 - 2,5 Cr, 20% Ni types. Scale resistance up to 1150 °C. No resistance in sulphuric environ-
3581-A: E > 29% Cr 25 - 27 ments. This alloy can withstand relatively severe thermal shock, and is superior to type
E 25 20 R 32 I > 70J (20 °C) Ni 20 - 22 309 L.
A 5.4: Si < 0,75 W.no:1.4823, 1.4826, 1.4828, 1.4832, 1.4840, 1.4841, 1.4846, 1.4848, 1.4837, 1.4710,
E 310-16 Mo < 0,75 1.4713, 1.4724, 1.4726, 1.4742, 1.4745, 1.4762, 1.4845, 1.4849
CEWELD 9606-1: FM5 T ~ 650 MPa C 0,06 - 0,2 4842 Kb is a basic electrode for welding heat-resistant austenitic steels of the 25% Cr,
4842 Kb Sect IX QW-432: F-No. 4 Y > 410 MPa Mn 1,0 - 2,5 20% Ni types. Scale resistance up to 1150 °C. No resistance in sulphuric environ-
3581-A: E > 29% Cr 25 - 27 ments. This alloy can withstand relatively severe thermal shock, and is superior to type
E 25 20 B 12 I > 70J (20 °C) Ni 20 - 22 309 L.
A 5.4: I > 32J (-196 °C) Si < 0,75 W.no: 1.4823, 1.4826, 1.4828, 1.4832, 1.4840, 1.4841, 1.4846, 1.4848, 1.4837, 1.4710,
E 310-15 Mo < 0,75 1.4713, 1.4724, 1.4726, 1.4742, 1.4745, 1.4762, 1.4845, 1.4849 heat resistant stain-
less steel, AISI 305, 310, 314, ASTM A297 HF, A297 HJ
CEWELD 9606-1: FM5 T ~ 600 MPa C 0,12 - 0,18 4850 Kb offers high corrosion resistance and excellent weldability on both AC and DC+.
4850 Kb 3581-A: Y > 380 MPa Cr 21 - 23 The weld deposit is scale resistant up to 1050 ºC.
~EZ 21 33 Nb B 32 E > 25% Ni 32 - 35 W.no: 1.4859 – GX10NiCrNb32-20; 1.4876 – X10NiCrAlTi32-20; X10NiCrAlTi32-20 –
I > 50J (20 °C) Nb 0,9 –1,2 Alloy 800 H, 1.4861
Mn ~ 4,5
CEWELD 9606-1: FM5 T ~ 700 MPa C 0,3 - 0,5 4853 Kb is suitable for joining and cladding high heat resistant CrNi-steels of the same
4853 Kb 3581-A: Y > 460 MPa Mn 0,9 - 1,1 kind and cast steels in a low sulphuric environment.
~EZ 25 35 Nb B 32 E > 8% Cr 25 - 27 W.no:1.4852, 1.4853 G-X 40 NiCrNb 35 25, 1.4857, G-X 40 NiCrSi 35 25, 1.4837,
Ni 34 - 36 G-X40CrNiSi25-12, 1.4848, G-X40CrNiSi25--20, 1.4849, G-X40NiCr38-18, G-
Si ~ 0,9 X40NiCrNb35-25, cast steels, HK40, HK45, UNS: J93503, J94204, N08705
Nb 1,2 -1,5
1/10