Micro and Surface Analysis in Art and Ar
Micro and Surface Analysis in Art and Ar
The various application possibilities of microscopic x-ray fluorescence and associated methods for the
characterization and provenance analysis of objects and materials of cultural heritage value are discussed
by means of a number of case studies. They include the trace analysis of historic glass, the analysis of
corroded coins and statues in bronze and silver and the study of inks on historical documents. These studies
are conducted by means of micro-XRF instruments installed at synchrotron beamlines and by means of
laboratory equipment, some of which is easily transportable to the museum or archaeological site where the
objects of interest are located. Copyright 2000 John Wiley & Sons, Ltd.
calcified tissues, paper and pigments by means of proton- a small beam, it is in general easier to select locations on
induced x-ray emission (PIXE) and related techniques is an object which resemble more closely to the ideal, flat
provided by Malmqvist.4 and polished surface normally required for reproducible
Since XRF meets a number of the above requirements, quantitative measurements.
analysis of objects of artistic and/or archaeological value A recent direction in -XRF instrument development is
with conventional XRF is fairly common; it is in fact one the construction of compact small-beam instruments, con-
of the most often applied methods for obtaining qualita- sisting for example of an air-cooled mini-focus x-ray tube,
tive and semi-quantitative information on the materials of a compact optical element for beam focusing/collimation
which these objects are made.5,6 On the other hand, the and a Peltier-cooled energy-dispersive detector. The avail-
use of conventional XRF for reliable quantitative analysis ability of such instruments, offering beams of 50–200 µm
is severely hampered by the fact that the irradiated area is cross-section, will be very useful for the in situ investi-
usually large. This prevents the separate analysis of details gation of archaeological and artistic materials, i.e. in the
of decorations, distinct features, etc. Also, the irradiation museum, gallery or archaeological site where they are nor-
geometry and sample surface are usually non-ideal and/or mally located.
not well defined, possibly introducing systematic errors in In this paper, after briefly describing the instrumentation
the quantification. The use of smaller x-ray beams can cir- employed for the investigations, a number of case studies
cumvent some of these limitations. In such as case, motor- highlighting the above-outlined types of investigations are
ized sample movement allows the local analysis capabil- outlined. Most of there were performed at the authors’
ity to be extended towards two-dimensional imaging of laboratories; the results of a number of other studies in
certain elements on the surface of artifacts. Since many the same field, taken from the literature, are briefly cited
objects of artistic and/or archaeological nature are fairly in order to complete the overview.
large and bulky (e.g. statues, oil paintings, vases, treasury
objects), instrumentation that can accommodate objects
of various shapes and is able to operate in air atmosphere MICRO-XRF EQUIPMENT EMPLOYED FOR
is very useful. Usually, this implies that the equipment INVESTIGATIONS IN ART AND
is laboratory-built as, for reasons of radiation protection, ARCHAEOMETRY
commercially available instruments mostly are equipped
with relatively small, well-shielded sample compartments.
Depending on the nature of the investigation and on the Synchrotron micro-XRF instrumentation
type of information required, one of the various forms of
-XRF may be employed. Polychromatic excitation at Hasylab Beamline L. The exper-
Synchrotron (-)XRF, offering ppm level detectability imental set-up used for synchrotron micro-XRF mea-
for many elements,7 can be used for quantitative fin- surements installed at Hasylab Beamline L in depicted
gerprint analysis of materials in order to gain a better schematically in Fig. 1(a). Figure 2(a) shows the energy
understanding of their provenance. The use of a micro- distribution in the white beam, produced in a bending
scopic beam permits the detailed investigation of the pro- magnet source, as seen through a 10 ð 10 µm pinhole,
cesses that have altered the surface composition of the positioned at 20 m from the synchrotron ring. As can be
material. Although suitable for trace-level microanalysis seen in Fig. 2(a), bending magnets of the DORIS storage
of organic materials (e.g. paper, pigments dispersed in a ring produce a white spectrum which contains apprecia-
organic binder) or for silicate-rich materials such as pot- ble amounts of very energetic photons (above 60 keV),
tery or glass, the high primary intensity of synchrotron which is not the case with many other synchrotron facili-
microbeams is usually not compatible with the analysis ties, e.g., the NSLS (National Synchrotron Light Source,
of metallic materials (e.g. artifacts made of bronze, iron, Upton, NY, USA).
silver, gold or alloys of these metals). The beam that originates from the storage ring is first
However, laboratory -XRF can be conveniently used collimated down to ca 100 ð 100 µm2 by motorized cross-
for this purpose. Another strong point of laboratory - slits before entering the capillary. The latter is mounted on
XRF is the possibility of performing local (quantitative) a motorized XYϕ stage for alignment to the beam. Usu-
analysis on objects whose size, shape or nature is incom- ally, straight borosilicate glass capillaries of 10–50 µm
patible with the vacuum and the small sample enclosures i.d. are employed for microbeam formation;9 the capil-
employed by most conventional microanalytical tech- lary–sample distance is typically of the order of a few
niques such as EPXMA and -PIXE. In this respect, - millimetres. Through repeated total external reflection on
XRF offers similar possibilities to external-beam PIXE,6 the inner walls of the tube, x-ray photons are transported
but with a better lateral resolution. along the length of the tubes; thus, straight capillaries act
Even for smaller objects (such as coins), which might as effective apertures over a wide energy range. Since
be analysed as a whole in a conventional XRF instrument, metal pinholes or cross-slit systems are not effective in
the use of a small beam instrument offers advantages collimating the high-energy portions of the white beam to
as only a small area of the (altered) surface needs to a micro-spot with well-defined shape, straight capillaries
be removed in order to expose the underlying original are employed for this purpose. However, these devices
material. A small x-ray beam obviously also permits the do not ‘concentrate’ the x-ray beam. If ellipsoidal lead-
analysis of an object at various locations, e.g. to verify glass capillaries are employed,10 the capillary is positioned
that all parts of a statue are made of the same material, or is such a way that its tip is about 0.5–1 mm away from
to investigate the homogeneity of the material used. XRF the sample surface. Inside ellipsoidal capillaries, the x-ray
on curved or otherwise non-flat surfaces can lead to errors photons are subject to only one or a few reflections and
in quantification (especially for metallic materials);8 with part of the radiation is focused in this manner. The sample
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 75
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
76 K. JANSSENS ET AL.
experimental facility is the fact that K-line XRF mea- beam spot of 3 ð 5 µm2 can be obtained. Because the
surements can be performed on the chemical elements monochromator is of the fixed-exit type, during XANES
ranging from K ⊲Z D 19⊳ to Pb ⊲Z D 82⊳ because of the energy scans, the position and width of the microbeam
high-energy components of the white beam. In the tran- on the sample do not change. This means that com-
sition metal range, femtogram-level absolute minimum pletely independently of each other, the irradiation posi-
detection limits (MDLs) in thin samples and ppm-level tion and primary beam energy can be user manipulated
relative MDLs in thick organic or silicate-based samples in a reproducible manner, permitting -XANES imag-
are obtained whereas for the lanthanides, equivalent val- ing. Such experiments involve normal XY scanning of the
ues are situated around 10 fg and 5–10 ppm, respectively, sample at various primary energies, as explained below
within a 1000 s irradiation time.15 In addition to the high (see Fig. 14).
intensity of the synchrotron beam, the high sensitivity over
an extended element rage is also the consequence of the
fact that in SRXRF spectra, a reduced background level Laboratory m-XRF equipment
is observed. This is the result of the polarized character
of the radiation and the fact that the XRF is detected in
Monocapillary-based m-XRF instrument. A schematic lay-
the plane of the synchrotron ring (see Ref. 16 for details).
out of a laboratory-scale -XRF spectrometer is shown
A disadvantage of the use of the strongly penetrating pri-
in Fig. 1(c). In principle, the basic layout is very simi-
mary and fluorescent radiation is that the analytical signals
lar to that of the polychromatic synchrotron instruments
in thick samples can originate from extensive depths [e.g.
described above. A glass capillary is used for concen-
for rare earth elements (REE) this can be up to several
trating the radiation generated by a rotating anode source
millimetres in glass samples], thereby reducing the effec-
on to the sample which is mounted on an XYZ stage.
tive lateral resolution of the technique in one direction.
The sample is viewed with an optical microscope using
This blurring effect can be avoided by employing thin
long working distance lenses. Elemental maps can be
samples.
recorded by moving the sample through the microbeam
and collecting an ED-XRF spectrum at each location.
Monochromatic excitation at the ESRF Beamline m-FID22. Since the efficiency with which conical and ellipsoidal
ESRF Beamline ID22 is an undulator beamline which capillaries concentrate x-rays decreases with increasing
means that instead of a continuous energy distribution photon energy, often Cr and/or Cu tubes are employed
such as shown in Fig. 2(a), only photons within spe- as x-ray sources in these instruments. With these tubes,
cific energy bands are produced. These relatively nar- beam sizes down to 5–10 µm can be employed with good
row (a few hundred eV wide) energy ranges are called sensitivity.8 When Mo or Rh anodes are used, the small-
undulator harmonics. Undulators are periodic multipole est beam size offering a sufficient photon flux is in the
magnetic structures of which the magnetic field strength range 20–40 µm. When comparing the elemental yields
can be adjusted to suit the users’ needs. Figure 2(b) (in counts s 1 pg 1 ) from this laboratory set-up and the
shows the energy spectrum of the undulator device at instrument at Hasylab Beamline L, a reduction by a factor
ESRF ID22. By changing the undulator gap width, the 10–30 in the elemental range Ca–Zr is noted. This means
energy of the harmonics can be adjusted so that the that all measurements take a long time to finish and auto-
output flux of an undulator in a specific energy range
mated overnight measurements are the rule rather than
can be optimized. In view of their quasi-monochromatic
the exception for image acquisition. Absolute MDL val-
nature, undulator sources are therefore more suitable for
ues in thin samples are situated in the 1–10 pg range as
performing micro-XRF experiments involving monochro-
opposed to femtogram levels with synchrotron instrumen-
matic primary microbeams, of which the energy can
tation. In addition, the advantages of the use of linearly
optionally be tuned. In Fig. 1(b), a schematic diagram
polarized synchrotron radiation with respect to spectral
of the experimental arrangement is shown. At ESRF
background reduction are not present here so that also in
ID22, a fixed-exit monochromator can be employed to
relative terms, the sensitivity is lower: in high scattering
select a very narrow energy band (E/E ³ 10 4 ) from
materials, typical detection limits in the 10–30 ppm range
an undulator peak. Via the monochromator settings, the
are obtained.
energy of the primary beam can be scanned in a nar-
row range around the absorption edge of an element of
interest in order to perform combined -XRF and - Polycapillary-based m-XRF spectrometer. The polycapillary
XANES (x-ray absorption near-edge spectroscopy). Dur- based -XRF spectrometer for which some results will be
ing a XANES experiment, the energy of the primary beam discussed below consists of a Kevex PXS4 mini-focus
is scanned in eV or sub-eV steps around an absorption Mo-tube x-ray tube (70 W maximum power, 250 µm
edge of a particular element while the absorption and/or anode spot), an XYZ sample translation/rotation stage,
the resulting flux of fluorescent radiation is measured. an optical microscope and an Si(Li) detector. The dis-
Since the exact location and shape of the absorption edge tance from the impact point of the electrons on the anode
changes as a function of the oxidation state and chem- to the Be window of the tube is ca 2.0 cm; the emerging
ical environment of the element in question, this type x-rays are focused by a polycapillary lens which is con-
of measurement can reveal information on the local oxi- tained in a cylindrical brass holder; the latter is mounted
dation state of that element. After the monochromator, on a five-axis gimbal lens holder (Newport M-LP-05B).
the beam is focused on to the sample by means of a The receiving end of the capillary is placed at a distance
Fresnel lens;17 an additional pinhole is used to reduce that maximizes the transmission through the lens. Fluores-
the scatter background in the sample area and to define cent radiation is detected with a 30 mm2 Canberra Si(Li)
the beam in the horizontal direction. In this manner, a detector (180 eV resolution at Mn K˛) having a 2.5 cm
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 77
Figure 3. Focusing characteristics of a polycapillary lens with Roman glass. Glass from the Roman period (1st–6th cen-
output focal length of 4.5 cm. The beam width is the smallest (ca
150 µm) at a distance of ca 42 mm from the end of the capillary turies) has a low magnesium/low potassium soda-lime
lens. composition,21 typically consisting of ca 66–72% SiO2 ,
16–18% Na2 O and 7–8% CaO. For Roman glass, the
diameter end-cap. In this case, a polycapillary lens manu- major element composition can only be used to verify
factured by the Institute for Low Energy Physics (Bejing that a particular fragment or object is genuinely Roman,
Normal University, Beijing, China) was employed. As but usually does not convey other information. The rea-
shown in Fig. 3, this lens focuses x-rays into a focal spot son for this is that all the glass found throughout the
of ca 150 µm at a distance of 4.5 cm from its output end. Roman Empire from the 1st to the 6th century features a
With lenses with shorter focal lengths (of ca 15 mm), focal nearly identical major element composition. As an exam-
spot sizes down to 50 µm were obtained. The most strik- ple, Table 1 gives the average composition of a number
ing advantage of using polycapillary lenses is that a large of glass fragments found at the Khirbet Qumrân site in
fraction of the cone of radiation that emerges from the Israel;22 in total, about 100 different objects of various
x-ray tube is collected by the lens. However, since the lens shapes were found at this site and analysed. In Fig. 4
mostly consists of strongly curved capillary tubes, its effi- the dendrogram obtained by hierarchical cluster analysis
ciency is must higher at low energy (below 10–15 keV) of the elemental data is shown. Two large groups may
than in the range 15–25 keV. Accordingly, this optical be discerned, of which the largest may be further subdi-
element strongly influences the excitation spectrum that vided. The average composition of the groups is given in
finally impinges on the sample surface.18 In the 5–10 keV Table 1. Comparison of the average compositions reveals
region of the spectrum, this gives rise to a high scatter a significant difference only in the CaO content (8% for
background but also to a high excitation efficiency. As a group 1 and 5% for group 2), which may be related to the
result, although a highly intense sub-millimetre beam can origin of the natron (an Na2 CO3 -rich deposit used a raw
be created in this way, the relative detection limits of this material for the glass making).
instrument for transition metals in glass are situated at the To verify the compositional homogeneity of the glass
30–100 ppm level. In metallic matrices such as bronze or in both groups, in addition to EPXMA measurements,
silver (strong matrix lines and strong self-absorption), the the trace compositions (down to the 1–10 ppm level) of
MDL values are around the 100 ppm level. the fragments were determined by -SRXRF. Details on
the calibration procedure applied and on its accuracy can
be found elsewhere.23 When also the trace concentrations
TRACE ELEMENT FINGERPRINTING are employed for performing a cluster analysis, the two
groups previously found are obtained, except that within
group 1 (Ca-rich), a subgroup containing five objects with
Trace analysis of ancient glass a much lower Sb concentration is identified (group 1b).
The distinction between groups 1 and 2 can now be made
Although not so frequently encountered at archaeological clearer since in the trace-element fingerprint, significant
sites as metallic and stone artifacts, the use of objects in differences in the average concentrations of Cu, Sn, Pb
silicate glass has been known since prehistoric times. Spe- and Sb are found. All these elements are associated with
cific glass compositions can be associated with particular the colour of the glass: Cu, Sn and Pb probably originate
time periods and geographical locations.19 It is recom- from bronze chips which may have been intentionally
mended to employ a microanalytical method to determine added to the glass melt to give it a green colour; Sb
the chemical compositions since only a minute piece of was used to decolorize the glass and give it a clear,
material is required for analysis. If the analyses are per- transparent appearance. Together, major and trace-element
formed on fragmented objects (as is mostly the case for data indicate that the entire series of ca 100 glass vessels
glass vessels found during excavations), sampling of small found at the Qumrân site originated from one or two
fragments of the material normally does not pose prob- workshops and were probably purchased together. This
lems. EPXMA can be used for major/minor element an- information supports the hypothesis24 that at this site
alysis down to ca 0.1% (w/w) (see, e.g., Ref. 20) but perfumes and ointments were manufactured on a large
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
78 K. JANSSENS ET AL.
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 79
Figure 4. Dendrogram obtained by clustering the major element data obtained from a number of the Qumrân glass artefacts. Two
large groups (1 and 2) are present; in their major composition, they differ significantly only in Ca content. Sample identification
numbers and vessel types are shown below the dendrogram.
that especially the Zr content of the glass can be used to The graph in Fig. 5(c) illustrates the usefulness of trace
distinguish between the glass vessels of Venetian and non- element data for making subtle compositional distinctions
Venetian origin found in Antwerp: whereas the majority of between cultural heritage artifacts of different provenance.
the Antwerp finds feature a ZrO2 content between 40 and By making use of the LURE microprobe, Figueiredo
100 ppm, the truely Venetian fragments and a very limited et al.35 characterized rare Mediterranean elongated glass
number of Antwerp finds show a significantly lower ZrO2 beads composed of five identifiable successive concentric
concentration in the range 10–20 ppm. layers of different colours: white, red, green and blue.
Figure 5. (a) Typical shapes, (b) Na2 O/CaO (%, w/w) and (c) Zr/Sr concentration scatter plots (ppm) of different types of 15–17th century
glass objects excavated in Antwerp, Belgium. The relative uncertainty is ca 5% on the major element concentrations is and ca 10% on
the trace concentrations. Circled fields in denote the majority of the genuinely Venetian ‘Cristallo’ and ‘Vitrum Blanchum’ objects.
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
80 K. JANSSENS ET AL.
Figure 5. (continued ).
They performed measurements at 8 and 21 keV primary only chromophore ion present) and therefore the redox
energy to optimize the excitation conditions for a large conditions during the manufacture of the glass determined
range of chemical elements. The incident synchrotron the colour of the glass. Additional research involving -
radiation was kept parallel to the bead axis to ensure that XANES to determine the oxidation state of Cu in the
all glass layers could be analysed separately. The white different layers is currently under way.
glass layers were opacified by means of Sn. Independently
of the colour, in each of the coloured layers significant
amounts of Cu and Pb were found, although the outer Analysis of inks
green layer is poorer in Pb and richer in Cu, K and Ca
relative to the other layers. The white and bluish layers The ability to analyse artifacts in an air environment
contain more Zn. Possibly the chemical state of Cu (the (i.e. without requiring vacuum) and in a non-destructive
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 81
manner makes -XRF especially suitable for the analy- for performing the large number of measurements required
sis of inks or other types of metal-containing pigmented to reveal systematic trends in the composition of paper and
materials deposited on fragile and easily damaged mate- inking.37
rials such as paper or parchment.
Visualization of invisible handwriting on historic documents.
Trace analysis of early printing inks. Knöchel and Haller36 In addition to SR-XRF, laboratory -XRF is also an excel-
and Mommsen et al.37 compared the concentrations of lent technique for the analysis of valuable documents, for
Cu and Pb in ink of the Gutenberg Bible with that of example to determine their authenticity. Typically, dif-
other early single leaf copies and books. The pioneering ferent inks, while having the same visible appearance,
work with PIXE by Cahill and co-workers38,39 identified will have different chemical compositions. Larsson43 and
the analysis of ink as a new research tool for the his- Stocklassa and Nillson44 described analysis by -XRF of
tory of early printing (from the second half of the 15th a 500-year-old Swedish possession letter (dated April l,
century).40,41 It is assumed that each printer/printing office 1499). The document, a sales contract for an estate,
can be recognized by a specific ink preparation as reflected showed signs of alterations. It was suspected that the alter-
in the trace element signature of the dried ink. The recipes ation was made in the 1530s, when the Swedish king
for the ink were kept as a secret; in the 15th century, not restored land back to certain nobles, who previously had
a single specification of composition is documented.42 been stripped of their estates by an earlier ruler. Although
Mommsen et al.37 employed a 0.5 ð 1 mm polychro- alteration was suspected by visual inspection (the origi-
matic x-ray beam derived from the synchrotron storage nal name of the owner had been removed by scraping),
ring ELSA (Bonn, Germany) for irradiating single leaves the original text was unreadable. By employing -XRF-
of early 15th century printed paper. Ink and paper of 22 generated Zn maps (a trace constituent of the original ink),
different works from different locations in Germany, Italy the original name could be established, however. In Fig. 6,
and Switzerland were analysed. The energy deposited in -XRF scans of Ca and Zn are shown across a selected
the paper during the measurements (300 s) was estimated area of the parchment. In the Ca map, the (falsified) visible
to be ca 15 µW cm 2 , i.e. about a factor of 70 lower than text can be seen, featuring the family name ‘Gäsmestad i
bright sunlight. Böre’; in the Zn map of the same area, however, a com-
Comparison of the spectra from paper and paper–ink pletely different text reading ‘Bøtinge i Asbo’ becomes
combinations from page II, 316 of the single leaf 42-line visible. Obviously, the forger used different ink for the
Gutenberg Bible revealed that Ni, Cu and Pb are present in alteration, accounting for the change in chemical makeup.
the ink at concentration levels of a few tens of µg cm 2 ,
whereas K, Ca, Ti, Mn, Fe and Zn originate from the
paper base. Local analysis of macroscopic objects
In six of the 22 leaves, printed areas could not be distin-
guished from blank areas, suggesting that the correspond- Enamel decorations. An area in which authentication of
ing inks were prepared from mainly C-bearing material art objects is of considerable (economical) interest in that
such as lampblack or soot.42 In some of the other inks, in of Oriental china ware. Up to the 17th century, high-
addition to Ni, Cu and Pb, also K, Ca and Fe were present. quality porcelain was exclusively manufactured in China
On all pages analysed except the Gutenberg leaf, the same and Japan and imported china ware was highly valued and
ink composition on the recto and verso sides were found. expensive. In the later periods an extensive production
On the recto side of the Gutenberg B-42 leaf, the ink system of counterfeit Chinese and/or Japanese porcelain
thickness was ca three times larger than on the verso side, both in Europe and in Asia came into existence. Some
although both sides show the same Cu/Pb and Ni/Pb ratios of the reproductions are very sophisticated and cannot
(1.0 š 0.5 and 0.007 š 0.003, respectively). For the same be easily distinguished from the original counterparts by
page (II, 316) of the Harvard Gutenberg Bible, by means visual inspection alone.
of PIXE recto and verso Cu/Pb ratios of 1.15 š 0.05 and Objective ways of distinguishing between original pe-
1.44 š 0.07, respectively were reported.37 – 40 riod and more contemporary reproductions have until
For three specific printers, the constancy of their ink now focused on the porcelain base material itself.34,35
composition over large time intervals was tested by A complementary approach is to consider the composi-
analysing leaves of several books produced by them. They tion of the enamel paints used to decorate the objects.
appear to have changed the composition of their inks fairly In view of the size and shape of the pieces, this type
frequently. It therefore appears difficult to establish a def- of analysis is difficult to perform using scanning elec-
inite trace element pattern specific for one printer. When tron microscopy equipped with energy-dispersive X-ray
only the trace elements which occur in the ink alone (and detection (SEM–EDX), while the intricacy of the deco-
not in the paper) are considered, only Pb and Cu con- ration patterns usually precludes the use of conventional
centrations can be used for distinguishing between early XRF. However, -XRF analysis of individual decorations
printers. is feasible.
As a result of this study, Mommsen et al.37 concluded As detailed earlier,9 by employing a monocapillary-
that a systematic investigation of the ink composition in based instrument, it is possible to record large-scale -
works printed 10–15 years after Gutenberg’s first Bible XRF maps of these decorations and to determine which
edition is needed to learn more about the early recipes transition elements (e.g. Mn, Fe, Cu) were employed to
for ink preparation and to find specific reasons for the colour the PbO-based enamel paint. As an example, Fig. 7
presence of metallic impurities in the ink. The SRXRF shows large-scale (4ð4 cm) x-ray maps of a painted figure
method was found to be suitable for non-destructive mea- on the vase shown in Fig. 8. To record these images, the
surements on this fragile type of material and appropriate vase was mounted on a rotation table so that surface of
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
82 K. JANSSENS ET AL.
Figure 6. Elemental maps of several elements obtained by -XRF analysis of an area on a Swedish property deed (photograph courtesy
of A. Rindby).
Figure 7. Large-area elemental maps obtained by translating/rotating a Japanese 18th century vase through a 15 µm beam. The area
scanned is 4 ð 4 cm.
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 83
the object maintained a constant distance to the capil- photons is 30 µm and at 35 keV it is 70 µm; 2 MeV protons
lary tip and detector. The various types of enamel paint penetrate about 12 µm in this material. Some of the quan-
[based on lead oxide as fluxing agent and coloured with titative data are shown in Fig. 9. Few differences in the
transition metals such as Fe (red), and Cu (green/black)] surface concentrations using the three beam methods were
can be clearly distinguished, in addition to the presence observed; however, a large discrepancy with the NAA
of decorative gold details. The K and Ca signals from the results was obtained. Compared with the bulk results, a
feldspar glaze are absorbed by the enamel paint. It appears very important enrichment of Ag together with a decrease
that originally these vases were only decorated with a few in Cu can be observed; this effect is especially important
simple blossoms (see Fig. 8, rightmost flower) but that for the Ag-rich coins.
later more decorations were added using enamel paint of Next to the Ag-enriched sub-surface layer, on top of
similar colour. It was possible to distinguish between orig- the upper surface of silver coins dark stains, enriched in
inally present and add-on decorations of the same colour Cu and other elements such as Fe, S and Cl, can also
on the basis of the local XRF spectra.9 occur. This may be the result of a heat treatment, causing
Coins and statues. Brissaud et al.45 compared SRXRF (as Cu from within the bulk to rise to the surface, because of
implemented in the LURE -XRF facility) at 17 and oxidation of the silver by atmospheric gases leading to the
35 keV excitation energy, PIXE and neutron activation formation of black Ag2 S or AgCl precipitates or simply
analysis (NAA) for the analysis of gallic coins having a as a result of mechanical wear and soiling during the use
Cu–Ag–Sn matrix composition. The aim of the investi- of the coins.
gation was to make a comparison of the data obtained To illustrate this, Fig. 10 shows elemental maps col-
from the surface of the coins with SRXRF and PIXE to lected with the polycapillary-based system from a Belgian
that obtained from the bulk of the samples with NAA. At silver coin of 1901, showing a royal portrait in relief. In
17 keV, in this matrix, the 1/e penetration depth of x-ray the Compton and Rayleigh maps, showing the variation
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
84 K. JANSSENS ET AL.
Figure 9. Quantitative data obtained from three Gallic coins by means of (a) SR-XRF at 17 keV primary energy (hatched bar), (b) at
35 keV (striped bar), (c) 2 MeV PIXE (full bar) and (d) neutron activation analysis (empty bar).
Figure 10. Optical photograph (left) and x-ray maps (right) of Cu, Ag and the scatter peak intensities obtained from a 19th century
Belgian silver coin. The scanned area is 10 ð 5 mm. The maps labelled ‘Compton’ and ‘Rayleigh’ show the variation of the scatter peak
intensities throughout the scanned area, highlighting the surface topology. Low intensity values are denoted by blue colours, medium
intensities by green and high intensities by red.
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 85
of the scatter peak intensity throughout the scanned area, (30–10 µm grain size) on the exposed area by means
the surface topology is clearly visible. At strongly curved of a rotating wooden rod, a smoothly polished area is
areas of the coin surface (facial features of portrait), where obtained [see Fig. 11(b)]. The polishing step was found
the take-off angle of the radiation towards the detector is to be required in order to improve the reproducibility
smaller than 45° , the absorption path of the scattered radi- of the analysis. A systematic study using the polycapil-
ation inside the metal is longer. Accordingly, these areas lary instrument revealed that this procedure allows one to
have a lower intensity in the scatter intensity maps. In the determine the Ag content in corroded coins with an accu-
Cu maps, an area showing a much higher Cu signal can racy of better than 1% provided that the measurements are
be seen; this area corresponds to a blackish stain on the performed in the centre of the circular depression shown
coin surface. In none of the different areas on the coin in Fig. 11(b).
however, was the correct Cu/Ag ratios found: inside the In the 19th century, great interest arose in the ancient
stain, the ratio is overestimated (too much Cu), while out- Egyptian civilization; many museums in the world cur-
side it, an excess of Ag is observed, even when the more rently own a collection of small Egyptian statues of a
penetrant Ag K radiation is used to determine the Ag con- religious nature in stone or bronze.47 To a varying extent,
tent. This necessitates the removal of some of the upper most metal statues have developed a corrosion layer that
surface layers to allow analysis of the underlying alloy. prevents reliable analysis of the Cu-based alloys from
Recently, the authors have evaluated a micro-polishing which the objects were made.48,49 This alteration layer
method in combination with -XRF analysis of the is much thicker (several tens to several hundreds of
exposed sub-millimetre sized surface for accurate deter- micrometres) than in the case of silver alloys. Never-
mination of the silver content in ancient Ag–Cu coins.46 theless, information on the original copper alloy is of
The procedure involves the use of a rotating stainless-steel interest since it can be used to trace the evolution of
grinding tool of sub-millimetre cross-section to remove Egyptian metallurgy in the period from 3000 BC to the
the upper, Ag-enriched surface layer in a very small area first century.50,51 Analyses of this type can also be used to
of the coin. The grinding step, which produces an unen- distinguish between original pieces and contemporary or
riched but fairly rough surface [see Fig. 11(a)], is followed earlier forgeries3 or to establish, for example, whether all
by a micro-polishing step. By applying diamond paste parts of a statue are made from the same alloy. By employ-
ing micro- or milli-beam XRF, several parts of a statue
can be examined under reproducible conditions (e.g. by
avoiding strongly curved surfaces), whereas for quantita-
tive analysis of the underlying metal, areas of the statue
which are corrosion free can be used. If these are not avail-
able, only small areas of the corrosion layer (e.g. on the
base of a statue) need to be removed, as explained above.
As an example, Table 2 lists quantitative analysis results
obtained from a statue of the god Nefer-hotep represented
in Fig. 12 (about 40 cm high, from the collection of the
Museum Vleeshuis, Antwerp, Belgium47 ) of exceptional
quality, dated to the XXII–XXIII dynasty (ca 1000 BC).52
It was analysed non-destructively by means of a simple
milli-XRF set-up consisting of a collimated low-power
mini-focus tube (70 W, 250 µm focal spot on Mo anode),
yielding a pencil beam of ca 300 µm diameter and a
30 mm2 Si(Li) detector. A fundamental parameter method
was used to obtain quantitative results. Analysis of brass
and bronze standards revealed that Cu, Zn, Sn and Pb
(the elements most informative on Cu metallurgy in this
period) could be determined with a relative accuracy of
ca 10% down to the 100 ppm level. The body of the
statue is copper coloured, has a very smooth surface and
shows only a very thin corrosion layer. The double crown
and base of the statue are darker in colour and have
a rougher texture, suggesting the presence of a thicker
corrosion crust and possibly the use of a different alloy
composition. Both crown and base were made separately
from the body. Since the data in Table 2 suggest a
difference in composition between the body of the statue
(legs, front of body) and its crown and base, on the
bottom side of the base, a few square millimetres of
the corrosion layer were polished away, exposing the
original metal. The results obtained after polishing are
also shown in Table 2 and indicate that there is in
Figure 11. Electron micrographs obtained after (a) micro-grin-
fact no large difference in composition between base
ding and (b) micro-grinding and micro-polishing of the surface and body and that probably all parts of the statue were
of an Ag–Cu alloy coin. made using a similar alloy composition and in the same
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
86 K. JANSSENS ET AL.
Table 2. Quantitative results (concentration, % w/w) local analysis of different locations on the statue shown in Fig. 12
Body
Crown Base (unpolished) Base (polished)
Right Head
Element leg Front band Lower Upper Front Back Bottom A Bottom A Bottom B Bottom C
Fe 0.12 0.14 0.25 0.09 0.09 0.11 0.11 0.15 0.09 0.07 0.08
Cu 81.2 82 76.5 72.8 75.8 72.6 70.7 71.4 80 84.9 84.8
Ag 0.05 0.04 0.12 0.18 0.13 0.17 0.19 0.13 0.07 0.06 0.06
Sn 13.7 12.9 14.8 19.8 17.5 22.3 21.6 21 15.3 12.2 12.2
Pb 4.8 4.5 7.6 6.5 6.2 4.3 7 6.7 4.6 2.5 2.5
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 87
Figure 13. (a) Backscattered electron micrograph of a corroded glass sample (cross-sectional view). The object was excavated at
Khirbet Qumrân, Israel. R, embedding resin; A, original glass; B, corroded layers, C, precipitation crust. The arrow indicates the location
of the line scan shown in (b). (b) Quantitative line profiles across the corrosion layer of a corroded Roman glass sample. A, original
glass; B, corrosion layer; C, precipitation crust on top of glass surface.
of trace constituents such as Cr, Ni, Cu, Zn, Pb, Bi, Sr asymmetric distribution and are enriched in the Mn-rich
and Mo. In Fig. 13(b), the quantitative line profiles are precipitation areas [the bright areas in Fig. 13(a)].
shown for a number of major, minor and trace elements These data, together with those obtained from other
across the corrosion layer, as obtained by -SRXRF. corroded glass samples, show that the corroded layer
Most trace elements are enriched in the corrosion layer, is not formed as the result of a simple, monotonous
with the exception of Sn, Sb and Zr that remain at leaching process during which the original major cations
the same level as in the bulk glass. For the tetravalent of the glass (NaC , Ca2C ) are replaced by others (KC ,
elements Sn and Zr this is not surprising since they take Mg2C ). Rather, a complex cycle of leaching followed by
part in the formation of the glass network; Sb behaves physical separation of the leached layer from the substrate
similarly to Sn, although some leaching is observed. Some glass, followed by renewed leaching, etc., must have
of the elements are enriched (K, Fe, Ti, Br) and show taken place. In the cavities between the different parts
a uniform distribution throughout the alteration layer. of the cracked-off layers, Mn can precipitate (presumably
Others elements, however, such as Cu and Bi [not shown in the MnO2 state), causing also other trace elements
in Fig. 13(b)], are concentrated on the boundary layer (present in the ground water) to become enriched in
between the original glass and corrosion or show an these areas.
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
88 K. JANSSENS ET AL.
Figure 13(c) shows the distribution of different elements Mn K radiation. At first sight, both Mn images indicate
throughout the corrosion body. However, in order to that in the scanning area, Mn enrichment has taken place
obtain a better understanding of the (various phases of) and that the spatial distribution of the Mn throughout
the corrosion process, this information should be comple- the corrosion layer is not well defined. However, when
mented by chemical information, i.e. localized information (after appropriate scaling) both Mn K intensity images
on the presence of certain elements in a particular chemi- are subtracted from each other [Mn (a) xMn (b)], an
cal state. In the case of the corroded glass, knowledge on image with much better contrast is obtained. The differ-
the distribution of various Mn species [such as Mn in the ence image corresponds to the contribution from Mn4C
2C (MnO), 3C (Mn2 O3 ) or 4C (MnO2 ) state] can con- (likely to be present as MnO2 ) and therefore represents
tribute significantly to insight into the corrosion mecha- a chemical Mn4C rather than an elemental Mn map. The
nism. Such information may be obtained by taking advan- scaling factor x was adjusted in such a way that the periph-
tage of the fact that the K-adsorption edge of Mn shifts eral areas of the difference map completely cancelled
over several eV towards higher energies with increasing out. The difference image clearly indicates that inside the
oxidation state. When Mn K˛ fluorescence is induced on successive layers itself of the corrosion body, no MnO2
the micro-scale by means of a focused, monochromatic crystal formation has taken place; MnO2 is exclusively
beam of which the energy can be changed within a certain confined to cavities between successive layers. This is an
range around the Mn K-edge position, while keeping the important conclusion since it may help direct the devel-
same position of the microbeam on the sample, localized opment of appropriate restoration treatments of corroded
XANES (x-ray absorption near edge structure) measure- glass (e.g. by the introduction of Mn-reducing fluids into
ments can be performed. In Fig. 14, x-ray maps obtained the cavities); also, during evaluation and intercomparison
by scanning a small (300 ð 300 µm) area on the sam- of alternative treatments, the effectiveness of the chem-
ple in Fig. 13(a) are shown. A monochromatic beam of ical transformations may be monitored in detail without
ca 3 ð 5 µm cross-section was employed. The measure- dissolution of the material itself.
ments were performed at the ID22 Beamline of ESRF. The
scanning range included an area which features a strong Combined m-XRF and m-XRD analysis of inclusions in iron
contract in the backscattered electron image of Fig. 13(a) artifacts. Dillman et al.56 studied inclusions in ferrous
and which also shows localized enrichment of Mn. The archaeological artifacts by using a combination of micro-
Si, Cl, K, Ca, Ti and one of the Mn images [Mn (b)] diffraction and micro-fluorescence at the LURE -XRF
were obtained by using a primary energy of 6.550 keV; station. For this purpose, a Bragg–Fresnel multilayer lens
at this energy, Mn in the 2C state is efficiently excited (BFML) was used to focus synchrotron radiation into a
(and will therefore produce Mn K fluorescent radiation) spot of a few square micrometres. Sixteen ferrous objects
whereas Mn in the 4C state is not. The other Mn image were studied, originating from the 1st, 5th and 17–19th
[Mn (a)] was obtained by repeating the scan at slightly centuries. Seven of the objects were manufactured using
higher energy (6.564 keV) so that also MnO2 (and other the ‘direct process’ to obtain iron from iron ore;57 the iron
Mn species in the 4C form) can contribute to the detected of the other nine objects was obtained by the ‘indirect’
Figure 14. Elemental maps of various elements obtained from a 300 ð 300 µm area on the sample shown in Fig. 13. A monochromatic
beam of ca 3 ð 5 µm cross-section was employed with tunable energy at the ESRF ID22 Beamline. The difference between the two Mn
images results in an ‘oxidation state’-specific map of Mn4C , present as MnO2 precipitates in the cavities between the successive layers
forming the corrosion body.
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 89
process. One of the investigated objects was a girder from to a few percent only) or from the clay lining of the
the Eiffel Tower in Paris. furnace. On the other hand, Al is known to be lower in
The direct process of iron reduction was employed concentration in cast iron which is obtained by means of
in low shaft furnaces in which the melting temperature the ‘indirect’ process.
of the iron is not reached. The resulting iron or steel
contains many non-metallic inclusions; from the 10th
century onwards, the ‘indirect process’ was developed, in Towards in situ m-XRF investigations
which the iron ore is heated to a much higher temperature
so that iron reduction takes place in the liquid phase; this Conventionally, ED-XRF is performed on relatively small-
also introduces carbon into the iron. In a second stage, scale but still stationary instruments. In direct excitation
the resulting cast iron (an alloy of Fe, Si and C) can be instruments, the major reason for the size and station-
refined by oxidation of the carbon. ary nature of the instrument is the presence of a bulky
The study of the inclusions trapped in the iron matrix Dewar vessel for cryogenic cooling of the solid-state
allows the identification of the type of reduction process detector. In the last 5 years, various efforts have been
employed and complements historic and iconographic data made to develop non-liquid nitrogen equivalents of the
on the evolution of these techniques.58 Si(Li) detector; a comprehensive review of these devel-
For the -XRF and -XRD measurements, the inclu- opments was given by Ellis et al.59 Some of these devices
sions were separated from the iron matrix in a multi-step are being used in commercially available or laboratory-
process.56 In Table 3, an overview is presented of the min- built compact XRF devices which may be used for on-site
eral phases that were identified in the inclusions of each investigations of archaeological and/or artistic materials.60
artifact; some of the inclusions were as small as 20 µm in Specific examples are the HgI2 detector which is incorpo-
diameter. rated into a radioisotope-based portable XRF instrument
In the materials obtained via the direct process, in all ca- (TN9000, Thermo Unicam, Cambridge, UK)61,62 and an
ses, aluminium-containing phases such as (Mg,Al)Fe2 O4 , Si-PIN detector (Amptek, Bedford, MA, USA).63 With
hyrcinite or galaxite are encountered in the inclusions. some of the devices, small beams (of ca 1 mm2 cross-
Fayalite (Fe2 SiO4 ) and wustite were also found. The section) may also be generated for local analysis.
latter minerals were also detected in the inclusions of the
materials obtained by means of the indirect process. Secondary target instruments. Cesareo et al.64 described
Dillman et al.56 suggested that the presence of the Al the use of different source–detector combinations for per-
minerals may be used to discriminate between the direct forming in situ analyses of works of art and illustrated
and the indirect processes. When the direct process is the capabilities of these instruments with analysis results
employed, Al can enter into the iron from the ore (up derived from bronze and gold objects, ceramics, faience
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
90 K. JANSSENS ET AL.
and porcelains and pigmented materials on illuminated of enamel paints on Chinese porcelain and for the quan-
manuscripts. Measurements were performed in the Museo titative analysis of genuine and counterfeit Indian brass
di Villa Guilia (Rome, Italy), the Museo Sanna (Sassari, statues from the 16th century. By using the lenses instead
Italy), the Museo de Antropologia and the Museo del of an equivalent collimator, an increase in intensity by a
Templo Major (Mexico City, Mexico) and the Museo de factor 7–20 was obtained. For the measurements, an Mo
la Ciudad (Havana, Cuba). Most of the instruments con- rotating anode, operated at relatively low power (10 mA,
sisted of a W-anode x-ray tube (Radiolight, 20–80 kV, 50 kV) was employed. These results indicate that in com-
5 mA), equipped with Ba or Mo secondary targets and bination with a 50 W mini-focus tube (where these lenses
either a liquid nitrogen-cooled Si(Li) or HPGe detector can capture a much larger fraction of the total flux that
or a compact Peltier-cooled Si-PIN or HgI2 detector. The exits from the tube) sub-millimetre beams of high inten-
authors claimed that since the heaviest element of interest sity can be readily obtained. Carpenter and co-workers.70
in archaeometric investigations is Ba (Ba K˛ at 32 keV), reported a factor of 44 intensity gain when a monolithic
the reduced quantum efficiency of the Si-PIN (of only polycapillary device was used to optimize the -XRF
300 µm thickness) does not present serious limitations. An instrument at the Oak Ridge Center for Manufacturing
energy resolution for the latter two detectors of 280 and Technology.
200 eV, respectively, was reported. They also described
the use of a collimated direct excitation set-up, consist-
ing of a low-power tube operated typically at 35 kV and CONCLUSIONS
0.3–0.5 mA of which the outgoing radiation is collimated
by a 2.5 mm diameter aperture. The use of this type
of device, sometimes in combination with near-infrared In this paper, the current possibilities and future potential
reflectometry for non-destructive pigment identification in of -XRF for the analysis and characterization of archae-
frescoes from the Roman and Renaissance period (includ- ological artifacts and objects of art have been discussed
ing Michelangelo’s Last Judgement in the Sistine Chapel, and illustrated with a number of selected examples. The
Rome) has been described by various authors.65 – 67 applications listed are not intended to be exhaustive; there
Lu et al.68 constructed a small-beam XRF spectrometer is a bias in the examples that were selected from the field
for the assay of precious metals in jewellery that utilizes a of experience of the laboratory of the authors.
0.5–1 mm2 collimated beam from a low-power x-ray tube In general, it is important to point out that the applica-
coupled to a high efficiency proportional counter detector. tion of analytical methods in the field of archaeology is
aimed at answering one or more questions derived from
human history or the history of art. Present-day concepts
Use of compact focusing optics. One step towards the real- in this particular field are very often based on theories that
ization of the use of small (i.e. sub-millimetre) beams are lacking any real experimental proof.
in compact, low-power set-ups is to use equally com- As in many other ‘problem-solving’ areas of research,
pact x-ray lenses. With 50 W tubes and apertures, the there exists no unique and fail-safe method that can be
primary beam needs to have a cross-section of at least applied for tackling such problems. Rather, a plethora of
300–500 µm to allow for measurements within reason- analytical methods should be considered for exploitation,
able counting times (500–1000 s per point). The fact that each of which has its own specific advantages and lim-
some polycapillaries only produce beams of 50–100 µm itations for the problem at hand. In particular, all these
diameter does not present a limitation in investigations methods take into account the specific drawbacks involved
where mostly sub-millimetre sized (or larger) features of in sampling and analysis of archaeological samples. The
macroscopic objects are analysed. The marked advantage most important drawback in this area of analysis is that
of polycapillary lenses over monocapillary concentrators very often the samples are unique or too valuable to be
resides with the fact that they form a focal spot at a con- destroyed or altered by sampling. This is a major rea-
siderable distance (several centimetres) from the end of son for the predilection for microanalytical methods in
the lens whereas with monocapillaries the smallest beam this area. The other and more fundamental reason for the
diameters are reached at the point where the beam leaves emphasis on microanalysis is that very often the sample
the capillary. This allows for a completely non-contact, which needs to be selected for analysis is microscopically
non-destructive kind of investigation and makes polycap- small, or the problem that needs to be addressed concerns
illary lenses ideal for local analysis of sensitive, precious a microscopic or extremely small volume.
and/or unique objects of macroscopic size such as statues, In this respect, -XRF offers a unique set of charac-
miniature paintings, coins, utilitarian objects in glass or teristics for solving many of the problems that arise. The
metal (goblets, vases, etc.) and the (often multi-coloured) method is completely non-destructive, can be applied to
decorations which are applied to them. Vekemans et al.69 minute sample amounts, sensitive, versatile and applicable
described the use of such devices for the local analysis to many materials.2
REFERENCES
1. P. T. Craddock and N. D. Meeks, Archaeometry 29, 187 3. F. Adams, A. Adriaens, A. Aerts, I. De Raedt, K. Janssens
(1987). and O. Schalm, J. Anal. At. Spectrom. 12, 257 (1997).
4. K. G. Malmqvist, in Particle Induced X-Ray Emission Spec-
2. Ch. Lahanier, G. Amsel, Ch. Heitz, M. Menu and H. H. Ander- trometry (PIXE), edited by S. A. Johansson, J. L. Campbell
sen, Nucl. Instrum. Methods Phys. Res. B 14, 1 (1986). and K. G. Malmqvist, Chapt. 7. Wiley, Chichester (1995).
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)
XRF NON-DESTRUCTIVE ANALYSIS IN ART AND ARCHAEOMETRY 91
5. S. A. Johansson and J. L. Campbell, PIXE: A Novel Technique 44. B. Stocklassa, G. Nillson, N. Paulson, paper presented at the
for Elemental Analysis. Wiley, Chichester (1988). European Conference on EDXRS, Myconos, Greece, May
6. A. M. Pollard and C. Heron, Archaeological Chemistry. Royal 30–June 6, (1992).
Society of Chemistry, Cambridge (1996). 45. I. Brissaud, J. X. Wang and P. Chevallier, J. Radioanal. Nucl.
7. F. Adams, K. Janssens and A. Snigirev, J. Anal. At. Spectrom. Chem. 131, 399 (1989).
13, 319 (1998). 46. I. Deryck and K. Janssens, Spectrochim. Acta, submitted for
8. M. Milazo and C. Cicardi, X-Ray Spectrom. 26, 211 (1997). publication.
9. K. Janssens, B. Vekemans, L. Vincze, F. Adams and 47. A. Oost (ed), Egypte Onomwonden. Catalogue of Egyptian
A. Rindby, Spectrochim. Acta, Part B 51, 1161 (1996). Artefacts of the Museum ‘Vleeshuis’, Antwerp (1995); (in
10. K. Janssens, L. Vincze, B. Vekemans, F. Adams, M. Haller Dutch).
and A. Knöchel, J. Anal. At. Spectrom. 13, 339 (1998). 48. L. Robbiola, I. Queixalos, L. P. Hurtel, M. Pernot and
11. L. Vincze, K. Janssens, F. Adams and K. W. Jones, C. Volfovsky, Stud. Conserv. 33, 205 (1988).
Spectrochim. Acta, Part B 50, 1481–1500 (1995). 49. L. Robbiola and C. Fiaud, Ed. Rev. Métall. 6, 156 (1993).
12. L. Vincze, K. Janssens, B. Vekemans and F. Adams, J. Anal. 50. M. Wuttmann, in Proceedings of the First International
At. Spectrom. 14, 529–533 (1999). Conference on Ancient Egyptian Mining and Metallurgy and
13. K. Janssens, L. Vincze, A. Aerts, F. Adams and J. Hertogen, Conservation of Metallic Artefacts, FIFAO, Cairo (1996).
X-Ray Spectrom. 26, 333 (1997). 51. M. Wuttmann, in Balat I, Le Mastaba de Medoe-Nefer,
14. A. Knöchel and M. Haller, J. Trace Microprobe Tech. 14, 461 Annexe III: Analyse et Étude du Métal Cuivreux de Certains
(1996). Objets, edited by M. Valloggia, 215–220. FIFAO 31/1, Cairo
15. K. Janssens, L. Vincze, B. Vekemans, C. T. Williams, (1986).
M. Radtke, M. Haller and A. Knöchel, Fresenius’ J. Anal. 52. G. Vittiglio, K. Janssens, B. Vekemans, F. Adams and A. Oost,
Chem. 363, 413–420 (1998). Spectrochim. Acta, Part B 54, 1697 (1999).
16. L. Vincze, K. Janssens, B. Vekemans and F. Adams, 53. J. Tate, Nucl. Instrum. Methods. Phys. Res. B 14, 20 (1986).
Spectrochim. Acta B 54, 1711 (1999). 54. E. Auer, Th. Rehren, A. von Bohlen, D. Kirchner and
17. B. Lai, B. Yun, D. Legnini, Y. Xiao, J. Chrzas, P. J. Vicaro, R. Klockenkamper, Metalla (Bochum) 5, 71 (1998).
V. White, S. Bajikar, D. Denton, F. Cerrina, E. Di Fabrizio, 55. K. Janssens, A. Aerts, L. Vincze, F. Adams, C. Yang,
M. Gentili, L. Grella and M. Baciocchi, Appl. Phys. Lett. 61, R. Utui, K. Malmqvist, K. W. Jones, M. Radkte, S. Garbe,
1877–1879 (1992). F. Lechtenberg, A. Knöchel and H. Wouters, Nucl. Instr.
18. N. Gao and D. Gibson, X-Ray Spectrom. 28, 75 (1999). Methods Phys. Res. B 109/110, 690 (1996).
19. E. V. Sayre and R. W. Smith, Science 133, 1824 (1961). 56. P. Dillman, P. Populus, P. Chevallier, P. Fluzin, G. Beranger
20. K. Janssens, I. Deraedt, O. Schalm and J. Veeckman, and A. Firsov, J. Trace Microprobe Tech. 15, 251 (1997).
Microchim. Acta. Suppl. 15, 253 (1998). 57. G. Magnusson (ed). The Importance of Iron Making, Techni-
21. B. Velde and G. Sennequier, Annales du 9 Congrés de cal Innovation and Social Change, Parts I and II. Proceedings
l’Association pour l’Histoire du Verre, 127–147 (1985). of the Norberg Conference, May 8–13, 1995. Jernkontorest
22. R. Donceel and P. Donceel-Voûte, Ann. N. Y. Acad. Sci. 772, Bergshistoriska Utskott, Stockholm (1995).
1 (1994). 58. D. Starley, in The Importance of Iron Making, Technical Inno-
23. A. Aerts, K. Janssens, F. Adams and L. Wouters, J. Arch. Sci. vation and Social Change, Parts I and II. Proceedings of the
26, 883 (1999). Norberg Conference, May 8–13, 1995, edited by G. Mag-
24. P. Donceel-Voûte, Archeologia 298, 24 (1994). nussen. Jernkontorest Bergshistoriska Utskott, Stockholm
25. B. Velde and C. Gedron, Archaeometry 22, 182 (1980). (1995).
26. B. Velde, Oxford J. Archaeol. 9, 105 (1990). 59. A. T. Ellis, P. J. Potts, M. Holmes, G. J. Oliver, C. Streli and
27. P. Hoffmann, Fresenius. J. Anal. Chem. 349, 320 (1994). P. Wobrauschek, J. Anal. At. Spectrom. 12, 461R (1997).
28. A. Aerts, PhD Thesis, University of Antwerp, (1998). 60. R. Cesareo, G. E. Gigante, I. S. Iwanczyk and A. Dabrowski,
29. R. G. Newton, Glass Technol. 21, 173 (1980). Nucl. Instrum. Methods. Phys. Res. A 380, 440 (1996).
30. E. V. Sayre, in Advances in Glass Technology, edited by 61. P. J. Potts, P. C. Webb, O. Williams-Thorpe and R. Kilworth,
F. R. Matson and G. E. Rindone, Vol. 2, p. 263–282. Plenum Analyst 120, 1273 (1995).
Press, New York (1963). 62. P. J. Potts, P. C. Webb and O. Williams-Thorpe, J. Anal. At.
31. B. Velde and A. Hochuli, Annales du 13 Congrès de Spectrom. 12, 769 (1997).
l’Association International pour l’Histoire du Verre, 185–192 63. A. C. Huber, J. A. Pantazis and V. T. Jordanov, in Proceedings
(1995).
of International Conference on Application of Accelerators
32. K. Janssens, I. Deraedt, O. Schalm and J. Veeckman,
in Research and Industry, Denton TX, 1994.
Microchim. Acta, Suppl. 15, 253 (1998).
64. R. Cesareo, G. E. Gigante, A. Castellano, M. A. Rosales,
33. K. H. Wedepohl, Die Herstellung Mittelalterlicher und
M. Aliphat, F. De La Fuente, J. J. Meitin, A. Mendoza,
Antiken Gläser. Steiner, Stuttgart (1993).
J. S. Iwanczyk and J. A. Pantazis, J. Trace Microprobe.
34. M. Verità and T. Tonianto, Riv. Staz. Sperimentale Vetro
Tech. 14, 711 (1996).
(Murano) 20, 169 (1990).
65. G. Fronterotta, S. Sciuti and M. Vendittelli, Proceedings of
35. M. O. Figueiredo, J. P. Veiga and T. Pereira da Silva, Proceed-
the 6th International Conference on ‘Non-Destructive Test-
ings of the 6th International Conference on ‘Non-destructive
ing and Microanalysis for the Diagnostics and Conservation
Testing and Microanalysis for the Diagnostics and Conser-
of the Cultural and Environmental Heritage,’ Rome, May
vation of the Cultural and Environmental Heritage,’ Rome,
17–20, 1999, pp. 257–270 (1999).
May 17–20, 1999, pp. 1769–1779 (1999).
36. A. Knöchel and M. Haller, J. Trace Microprobe Tech. 14, 461 66. S. Sciuti, in Proceedings of the 6th International Conference
(1996). on ‘Non-Destructive Testing and Microanalysis for the Diag-
37. H. Mommsen, Th. Beier, H. Dittmann, D. Heimermann, nostics and Conservation of the Cultural and Environmental
A. Hein, A. Rosenberg, M. Boghardt, E.-M. Manebutt-Benz Heritage,’ Rome, May 17–20, 1999, pp. 401–415, (1999).
and H. Halbey, Archeometry 38, 347 (1996). 67. N. Gabrielli and F. Morresi, in Proceedings of the 6th
38. T. Cahill, B. Kusko and R. N. Schwab, Nucl. Instrum. International Conference on ‘Non-Destructive Testing and
Methods. Phys. Res. B 181, 205 (1981). Microanalysis for the Diagnostics and Conservation of the
39. T. Cahill, B. Kusko, R. A. Eldred and R. N. Schwab, Cultural and Environmental Heritage,’ Rome, May 17–20,
Archaeometry 26, 3 (1984). 1999, pp. 2133–2139, (1999).
40. R. N. Schwab, Library Trends 36, 53 (1987). 68. R. Lu, A. Le, Y. Gu, G. Wu and J. Zhu, Nucl. Instrum. Methods.
41. R. N. Schwab, T. A. Cahill, B. H. Kusko, R. A. Eldred, G. Moller Phys. Res. B 104, 595 (1995).
and D. Dutschke, Pap. Bibliogr. Soci. Am. 8, 305 (1986). 69. B. Vekemans, K. Janssens, G. Vittiglio, F. Adams, L. Andong
42. C. H. Bloy, A History of Printing Ink, Balls and Rollers and Y. Yiming, Adv. X-Ray Anal. 41, 278 (1998).
1440–1850. Buttersworth, London (1967). 70. N. Gao, I. Ponomarev, Q. F. Xiao, W. M. Gibson and
43. S. Larsson, Thesis, Department of Physics, Chalmers Uni- D. A. Carpenter, Adv. X-Ray Anal. 39, 81 (1996).
versity of Technology, Goteborg. Bibliotekets ReproService,
Goteborg (1991).
Copyright 2000 John Wiley & Sons, Ltd. X-Ray Spectrom. 29, 73–91 (2000)