Pessing Libya INC: Fill: SMAW Sfa. No: 5.28&5.5 Post Weld Heat Treatment: 620-650 Deg C
Pessing Libya INC: Fill: SMAW Sfa. No: 5.28&5.5 Post Weld Heat Treatment: 620-650 Deg C
WELDING DETAILS
Weld
Weld Filler Voltage Heat
Pass process ΦD Current (A) Polarity Speed
Layer Material (V) Input
Cm/min
1 Root GTAW ER70S-A1 mm 2.4 60-90 10-11 DCEN N/A N/A
2 Fill SMAW E7018-A1
mm 2.5,3.25 70-130 22-25 DCEP N/A N/A
Inspection Code or Standard: ANSI B31.3
Inspection Magnetic Particle or Radiographic Test or Pressure
Visual
Method Dye Penetrant Ultrasonic Test Test
Extent of UT:
100% MT: 100% PT: 100% RT: 10% YES
Examination 10%
WELDING AND POST WELDING HEATTREATMENT
Preheat Temperature: 150 deg c Thermal Design Drawing No.: N/A Post Heat Treatment:620-650 deg c
Inspection: RTG-10%
Prepared by: Eng. Mahmoud Helmy Approved by: Eng. Walid Saad Witnessed by: WABAG
AWS/CWI certification no.: (21097031) QC Head section
:Signature :Signature
Date: 21. 12. 2021 Date: 21. 12. 2021 :Date