TEK 01-01F

ASTM SPECIFICATIONS FOR CONCRETE


MASONRY UNITS

INTRODUCTION

The most widely-used standards for specifying concrete masonry units in the United States
are published by ASTM International. These ASTM standards contain minimum
requirements that assure properties necessary for quality performance. These requirements
include items such specified component materials, compressive strength, permissible
variations in dimensions, and finish and appearance criteria. Currently, seven ASTM
standards apply to units intended primarily for construction of concrete masonry walls,
beams, columns or specialty applications (see Table 1).
The letter and first number of an ASTM designation is the fixed designation for that
standard. For example, ASTM C55 is the fixed designation for concrete building brick. The
number immediately following indicates the year of last revision (i.e., ASTM C55-11 is the
version of C55 published in 2011). A date in parentheses after the last revision date is the
reapproval date.

Because significant changes can be introduced into subsequent editions, the edition
referenced by the building code or by a project specification can be an important
consideration when determining specific requirements. Also note that it may take several
years between publication of a new ASTM standard and its subsequent reference by a
building code. For this reason, Table 1 includes the editions referenced in the 2006, 2009
and 2012 editions of the International Building Code (IBC) (ref. 1), as well as the most current
ASTM edition. Code officials will commonly accept more current editions of ASTM
standards than that referenced in the code, as they represent state-of-the-art requirements.

Page 1
 Table 1—ASTM Specifications for Concrete Masonry Units

A Although not directly referenced in the IBC, C129 is


referenced in Specification for Masonry Structures (ref. 2)
B This standard is not referenced in the IBC.

LOADBEARING CONCRETE MASONRY UNITS— ASTM C90

As the most widely-referenced ASTM standard for concrete masonry units, ASTM C90 is
under continuous review and revision. The bulk of these revisions are editorial, although
two recent major changes are discussed here.

In 2011, web thickness requirements were significantly revised. Prior to ASTM C90-11b (ref.
3), there were different minimum web thicknesses based on unit width. Additionally,
equivalent web thickness, a measure of the width of web per foot of wall length was used to
determine if sufficient web was present to transfer shear loads. In ASTM C90-11b, these
requirements were replaced with a single minimum web thickness (0.75 in., 19.1 mm),
regardless of unit width. The equivalent web thickness was replaced with a normalized web
area, a measure of the area of web contact with the face shells per square foot of wall (see
Table 2).

In 2000, the Type I (moisture-controlled) and Type II (non moisture-controlled) unit


designations were removed from C90. The designations were withdrawn because they were
difficult to effectively use and enforce, and because of newly developed concrete masonry
crack control provisions. The new crack control guidelines are based on anticipated total
volume changes, rather than on the specified moisture contents that formed the basis for
Type I requirements. Control joint criteria can be found in References 5 and 6. For more
detailed information on removal of the Type designations, see the Frequently Asked
Question on this topic here.

Page 2
 Table 2—ASTM C90-11b Minimum Face Shell & A Web Requirements for Hollow
Units (ref. 3)

A Average of measurements on a minimum of 3 units when


measured as described in Test Methods C140 (ref. 4).

B For units with split surfaces, a maximum of 10% of the split


surface may have thickness less than those shown, but not less
than ¾ in. (19 mm). When the units are to be solid grouted,
the 10% limit does not apply and Footnote C establishes a
thickness requirement for the entire face shell.

C When the units are to be solid grouted, minimum face shell


and web thickness shall be not less than ⅝ in. (16 mm). D
Minimum normalized web area does not apply to the portion of
the unit to be filled with grout. The length of that portion
shall be deducted from the overall length of the unit for the
calculation of the minimum web cross-sectional area.

Physical Requirements

Physical requirements prescribed by ASTM C90 include dimensional tolerances, minimum


face shell and web thicknesses for hollow units, minimum strength and maximum
absorption requirements, and maximum linear shrinkage.

Overall unit dimensions (width, height and length) can vary by no more than ±⅛ in. (3.2
mm) from the standard specified dimension. Exceptions are faces of split-face units and
faces of slump units which are intended to provide a random surface texture. In these cases,
consult local suppliers to determine achievable tolerances.

Page 3
Molded features such as rib and scores must be within ±1⁄16 in. (1.6 mm) of the specified
dimension 1 and within ±1⁄16 in. (1.6 mm) of the specified placement on the mold. For dry-
stack masonry units, the physical tolerances are typically limited to ±1⁄16 in. (1.6 mm), which
precludes the need for mortaring, grinding of face shell surfaces or shimming to even out
courses during construction (ref. 7).

Minimum face shell and web thicknesses are those deemed necessary to obtain satisfactory
structural and nonstructural per- formance. Note that although there are some unique face
shell thickness requirements for split-faced units (see Table 2 footnote B), ground-face units
(i.e., those ground after manufacture) must meet the face shell thickness requirements
contained in the body of Table 2. In addition to minimum permissible web thicknesses for
individual webs, the specification also requires a minimum total web contact area with face
shells per square foot of wall area. When evaluating this normalized web area, the portion of a
unit to be filled with grout is exempted. This provision avoids excluding units intentionally
manufactured with reduced webs, including bond beam units and open-end block, where
grout fulfills the structural role of the web.

A solid unit is one with a net cross-sectional area in every plane parallel to the bearing
surface of at least 75% of the gross cross-sectional area measured in the same plane.
Minimum face shell and web thicknesses are not prescribed for solid units.

The net area used to determine compressive strength is the “average” net area of the unit,
calculated from the unit net volume based on tests described in ASTM C140 (ref. 4). Gross
and net areas are shown in Figure 1.

Net area compressive strength is used for engineered masonry design, taking into account
the mortar bedded and grouted areas. Gross area compressive strength is still used for
empirically designed masonry (IBC Section 2109).

Maximum permissible water absorption is shown in Table 3. Absorption is a measure of the


total water required to fill all voids within the net volume of concrete. It is determined from
the weight-per-unit-volume difference between saturated and oven-dry units. Aggregates
with relatively large pores, such as some lightweight aggregate, have a greater absorption
than dense, nonporous aggregates, given the same compaction. As a result, lightweight units
are permitted higher absorption values than medium or normal weight units.

Because concrete masonry units tend to contract as they dry, C90 limits their potential
drying shrinkage to 0.065%, measured using ASTM C426 (ref. 8).

Page 4
 Figure 1—Gross and Net Areas

 Table 3—Strength and Absorption Requirements for Concrete Masonry Units,


ASTM C90 (ref. 3)

Finish and Appearance

Finish and appearance provisions prohibit defects that would impair the strength or
permanence of the construction, but permit minor cracks incidental to usual manufacturing
methods. For units which will be exposed, the presence of objectionable imperfections is
based on viewing the unit face(s) from a distance of at least 20 ft (6.1 m) under diffused
lighting. Five percent of a shipment may contain chips not larger than 1 in. (25.4 mm) in any
dimension, or cracks not wider than 0.02 in. (0.5 mm) and not longer than 25% of the
nominal unit height. The specification requires that color and texture be specified by the
purchaser.

An approved sample of at least four units, representing the range of color and texture
permitted, is used to determine conformance.

Page 5
CONCRETE BUILDING BRICK—ASTM C55

ASTM C55-03 (ref. 9a) included two grades of concrete brick: Grade N for veneer and facing
applications and Grade S for general use. In 2006, the grades were removed and
requirements for concrete brick used in veneer and facing applications were moved into a
new standard: C1634 (see below). ASTM C55 now only applies to concrete masonry units
with: a maximum width of 4 in. (102 mm); a weight that will typically permit it to be lifted
and placed using one hand; and an intended use in nonfacing, utilitarian applications.

Requirements for C55-11 (ref. 9b) units include:

2,500 psi (17.2 MPa) minimum compressive strength (average of three units),

0.065% maximum linear drying shrinkage,

75% minimum percent solid, and

maximum average absorption requirements of 13 pcf for normal weight brick, 15 pcf for
medium weight brick and 18 3 pcf for lightweight brick (208, 240 and 288 kg/m ).

Finish and appearance criteria only address defects which might affect placement or
permanence of the resulting construction.

CONCRETE FACING BRICK—ASTM C1634

A facing brick (C1634) is distinguished from a building brick (C55) primarily by its intended
use: a facing brick is for uses where one or more unit faces will be exposed.
Compression and absorption requirements are listed in Table 4. Linear drying shrinkage,
dimensional tolerances and finish and appearance requirements are similar to those in C90,
with the exception that chip size is limited to ±½ in. (13 mm). Both C1634 and C55 refer to
C140 (ref. 4) for compression testing, which requires compression test specimens to have a
height that is 60% + 10% of its least lateral dimension, to minimize the potential impact of
specimen aspect ratio on tested compressive strengths.

 Table 4—Strength and Absorption Requirements for Concrete Facing brick, ASTM
C1634 (ref. 10)

Page 6
NONLOADBEARING CONCRETE MASONRY UNITS— ASTM C129

ASTM C129 (ref. 11) covers hollow and solid nonloadbearing units, intended for use in
nonloadbearing partitions. These units are not suitable for exterior walls subjected to
freezing cycles unless effectively protected from the weather. These units must be clearly
marked to preclude their use as loadbearing units. Minimum net area compressive strength
requirements are 500 psi (3.45 MPa) for an individual unit and 600 psi (4.14 MPa) average
for three units.

CALCIUM SILICATE FACE BRICK—ASTM C73

ASTM C73 (ref. 12) covers brick made from sand and lime. Two grades are included:

Grade SW—Brick intended for exposures below freezing in the presence of moisture.
Minimum compressive strength requirements are 4,500 psi (31 MPa) for an individual unit
and 5,500 psi (37.9 MPa) for an average of three units, based on average gross area. The
maximum water absorption is 15 lb/ft3 (240 kg/m3).

Grade MW—Brick intended for exposure to temperatures below freezing, but unlikely to
be saturated with water. Minimum compressive strength requirements are 3,000 psi (20.7
MPa) for an individual unit and 3,500 psi (24.1 MPa) for an average of three units, based on
average gross area. The maximum water absorption is 18 lb/ft3 (288 kg/m3).

PREFACED CONCRETE AND CALCIUM SILICATE MASONRY UNITS—ASTM


C744

ASTM C744 (ref. 13) establishes requirements for the facing materials applied to masonry
unit surfaces. For the units onto which the surface is molded, C744 requires compliance with
the requirements contained in ASTM C55, C90 or C129, as appropriate. Facing requirements
in C744 include: resistance to crazing, surface burning characteristics, adhesion, color
permanence, chemical resistance, cleansability, abrasion, and dimensional tolerances.

CONCRETE MASONRY UNITS FOR CATCH BASINS AND MANHOLES—ASTM


C139

ASTM C139 (ref. 14) covers solid precast segmental units intended for use in catch basins and
manholes. Units are required to be at least 5 in. (127 mm) thick, with a minimum gross area
compressive strength of 2,500 psi (17 MPa) (average of 3 units) or 2,000 psi (13 MPa) for an
individual unit, and a maximum water absorption of 10 pcf (16 kg/m³) (average of 3 units).
The overall unit dimensions must be within ± 3% of the specified dimensions.
Page 7
References
1. International Building Code. International Code Council, 2006, 2009, 2012.

2. Specification for Masonry Structures, TMS 602-11/ACI 530.1-11/ASCE 6-11. Reported by


the Masonry Standards Joint Committee, 2011.

3. Standard Specification for Loadbearing Concrete Masonry Units, ASTM C90-11b. ASTM
International, 2011.

4. Standard Test Methods for Sampling and Testing Concrete Masonry Units and Related
Units, ASTM C140-11b. ASTM International, 2011.

5. Control Joints for Concrete Masonry Walls—Empirical Method, TEK 10-2C. National
Concrete Masonry Association, 2010.

6. Control Joints for Concrete Masonry Walls—Alternative Engineered Method. TEK 10-3.
National Concrete Masonry Association, 2003.

7. Design and Construction of Dry-Stack Masonry Walls, TEK 14-22. National Concrete
Masonry Association, 2003.

8. Standard Test Method for Linear Drying Shrinkage of Concrete Masonry Units, ASTM
C426-10. ASTM International, 2010.

9. Standard Specification for Concrete Brick, ASTM C55. 9a. ASTM C55-03, ASTM
International, 2003. 9b. ASTM C55-11, ASTM International, 2011.

10. Standard Specification for Concrete Facing Brick, ASTM C1634-11. ASTM International,
2011.

11. Standard Specification for Nonloadbearing Concrete Masonry Units, ASTM C129-11. ASTM
International, 2011.

12. Standard Specification for Calcium Silicate Brick (Sand-Lime Brick), ASTM C73-10. ASTM
International, 2010.

13. Standard Specification for Prefaced Concrete and Calcium Silicate Masonry Units, ASTM
C744-11. ASTM International, 2011.

14. Standard Specification for Concrete Masonry Units for Construction of Catch Basins and
Manholes, ASTM C139-11. ASTM International, 2011.

NCMA TEK 01-01F, Revised 2012

Disclaimer: Although care has been taken to ensure the enclosed information is as
accurate and complete as possible, NCMA does not assume responsibility for errors

Page 8
or omissions resulting from the use of this TEK.

Keywords

absorption ASTM specifications compressive strength concrete brick

dimensions face shell thickness gross area net area specifications

testing water absorption web thickness

Page 9