SA-517 Grade A, B, E, F, H, P, Q, S

Overview
This quenched and tempered grade is used primarily in pressure vessel applications.
The elevated physicals of this alloy grade is applicable for environments where
added strength is required.

Chemical Requirements
*Elements represented in percentage

Elements Grade A % Grade B % Grade E % Grade F % Grade H % Grade P % Grade Q % Grade S %


Carbon
Heat
0.15-0.21 0.15-0.21 0.12-0.20 0.10-0.20 0.12-0.21 0.12-0.21 0.14-0.21 0.10-0.20
analysis
Product
0.13-0.23 0.13-0.23 0.10-0.22 0.08-0.22 0.10-0.23 0.10-0.23 0.12-0.23 0.10-0.22
analysis
Manganese
Heat
0.80-1.10 0.70-1.00 0.40-0.70 0.60-1.00 0.95-1.30 0.45-0.70 0.95-1.30 1.10-1.50
analysis
Product
0.74-1.20 0.64-1.10 0.35-0.78 0.55-1.10 0.87-1.41 0.40-0.78 0.87-1.41 1.02-1.62
analysis
Phosphorus,
0.025 0.025 0.025 0.025 0.025 0.025 0.025 0.025
max
Sulfur, max 0.025 0.025 0.025 0.025 0.025 0.025 0.025 0.025
Silicon
Heat
0.40-0.80 0.15-0.35 0.10-0.40 0.15-0.35 0.15-0.35 0.20-0.35 0.15-0.35 0.15-0.40
analysis
Product
0.34-0.86 0.13-0.37 0.08-0.45 0.13-0.37 0.13-0.37 0.18-0.37 0.13-0.37 0.13-0.45
analysis
Nickel
Heat
– – – 0.70-1.00 0.30-0.70 1.20-1.50 1.20-1.50 –
analysis
Product
– – – 0.67-1.03 0.27-0.73 1.15-1.55 1.15-1.55 –
analysis
Chromium
Heat
0.50-0.80 0.40-0.65 1.40-2.00 0.40-0.65 0.40-0.65 0.85-1.20 1.00-1.50 –
analysis
Elements Grade A % Grade B % Grade E % Grade F % Grade H % Grade P % Grade Q % Grade S %
Product
0.46-0.84 0.36-0.69 1.34-2.06 0.36-0.69 0.36-0.69 0.79-1.26 0.94-1.56 –
analysis
Molybdenum
Heat
0.18-0.28 0.15-0.25 0.40-0.60 0.40-0.60 0.20-0.30 0.45-0.60 0.40-0.60 0.10-0.35
analysis

Tensile Requirements
2.50 in. [65 mm] and Over 2.50 to 6 in. [65
Under to 150 mm]
Tensile strength 115-135 [795-930] 105-135 [725-930]
Yield strength, min, ksi [MPa] 100 [690] 90 [620]
Elongation in 2 in. [50 mm], min, % 16 14
Reduction of area, min, %:
Rectangular specimens 35 –
Round specimens 45 45