WELD REPAIR ANALYSIS
Tabel 3 : The defects of each welder is tabulated below.
Date From:
Date To:
Cummulative This Period Defects analysed-This Period
Repair
Welder Jnts RT/ UT RT/ UT Total Welding
Welded Done
Repair Rep% Jnts Welded
Done
Repair Rep% EP IP LOF P RC UC JOINT SIZE Material
Reject Process
BSCW-130 552 251 17 6.77 % 5 19 2 10.53 % 2 2 2 LTCS & SS_SOUR GTAW
BSCW-156 530 225 8 3.56 % 9 1 1 100.00 % 1 1 2 INCOLOY825 GTAW
BSCW-165 133 115 2 1.74 % 0 1 1 100.00 % 1 1 12 CS GTAW
BSCW-185 383 103 5 4.85 % 1 8 1 12.50% 1 1 3 SS_SOUR GTAW
BSCW-240 213 80 3 3.75 % 5 1 1 100.00 % 1 1 0.75 SS_SOUR GTAW
BSCW-297 203 117 6 5.13 % 7 15 2 13.33 % 1 1 2 4" & 6" CS & LTCS GTAW
BSCW-298 87 50 3 6.00 % 4 9 1 11.11 % 1 1 4 LTCS GTAW
BSCW-300 257 43 3 6.98 % 4 2 2 100.00 % 1 1 2 0.75" & 0.75" CS_SOUR GTAW
BSCW-316 150 24 3 12.50 % 6 5 1 20.00 % 1 1 2 CS GTAW
BSCW-330 44 11 1 9.09 % 3 4 1 25.00 % 1 1 2 LTCS GTAW
BSCW-354 71 47 3 6.38 % 2 2 1 50.00 % 1 1 0.75 LTCS_SOUR GTAW
BSCW-406 54 47 4 8.51 % 3 10 1 10.00 % 1 1 12 CS GTAW
BSCW-410 36 33 3 9.09 % 4 18 3 16.67 % 2 1 3 2", 2" & 4" CS & LTCS GTAW
BSCW-422 45 28 5 17.86 % 2 8 2 25.00 % 2 2 12" & 12" LTCS GTAW
BSCW-425 32 29 6 20.69 % 1 9 2 22.22 % 2 2 4" & 4" LTCS GTAW
TOTAL 22 1 1 11 5 3 1 22
Page 1 of 1