HASTELLOY® C-22HS™alloy
HASTELLOY® C-22HS™alloy
HASTELLOY® C-22HS™alloy
Corrosion-Resistant Alloys
Contents Principal Features Chemical Composition Physical Properties Corrosion Data Iso-Corrosion Diagrams Mechanical Properties Welding and Fabrication Fabrication Health and Safety
3 3 4 5 8 10 13 14 15
H-2122
A TEM darkfield image of C-22HS alloy in the age-hardened condition. The lighter colored particles are Ni2(Mo,Cr) precipitates on the order of 10 nm in diameter which give the alloy its high strength. Also shown (inset) is a [001] diffraction pattern indicating that the crystal structure of the precipitates is of the Pt2Mo type.
Plot illustrating the unique combination of high strength and high corrosion resistance of C-22HS alloy.
PRINCIPAL FEATURES
Outstanding Corrosion Resistance, High Strength HASTELLOY C-22HS TM alloy** is corrosion-resistant, nickel-chromium-molybdenum alloy which can be heat treated to obtain a strength approximately double that of other C-type alloys. Importantly, the corrosion resistance and ductility of the alloy remain excellent when in the high strength condition. In addition to its high uniform corrosion resistance in oxidizing as well as reducing environments, the as-heat treated C-22HS alloy possesses high resistance to chloride-induced pitting and crevice corrosion attack. Product Forms C-22HS alloy is available in the form of plate, sheet, strip, billet, bar, wire, pipe, and tube. Heat Treatment The high strength of C-22HS alloy is derived from the formation of strengthening particles of Ni2 (Mo,Cr) which form during the patented*** two-step age-hardening heat treatment. The approximately 48 hour heat treatment, 1300F (705C) FC to 1125F (605C)/32 hours/AC, is described in more detail on page 14. Solution Annealed and Filler W ire Applications C-22HS alloy may also be considered for applications which do not require the high strength imparted by the heat treatment. In the annealed condition, C-22HS alloy has even higher corrosion-resistance, particularly with regard to localized corrosive attack. This localized attack resistance also makes the alloy an attractive candidate as a general-purpose filler metal or weld overlay. Applications Agitators and blenders Shafting Fan blades and hubs Fasteners Springs Valves Dies Screws W ellhead parts Rings and gaskets
Field Test Program Samples of C-22HS alloy in the age-hardened condition are available for field trials. Furthermore, samples can be weighed prior to delivery, and then reweighed after test by the customer, and reports provided on corrosion rates and other observations. For samples, please contact one of the Haynes International Service Centers listed on the back cover of this brochure. ** Covered by U.S. Patent 6,860,948 *** Covered by U.S. Patents 6,544,362 and 6,638,373
COMPOSITION
Ni BAL Cr 21 Mo 17 Fe 2* Co 1* W 1* Mn 0.8* Al 0.5* Si C B 0.08* 0.01* 0.006*
*Maximum 3
HASTELLOY C-22HS alloy
PHYSICAL PROPERTIES*
Physical Property Density (annealed) Density (age-hardened) Electrical Resistivity RT RT RT 100C 200C 300C 400C 500C 600C RT 100C 200C 300C 400C 500C 600C 25-100C 25-200C 25-300C 25-400C 25-500C 25-600C RT 100C 200C 300C 400C 500C 600C RT 100C 200C 300C 400C 500C 600C RT 100C 200C 300C 400C 500C 600C Metric Units 8.60 g/cm. 8.64 g/cm. 0.98 ohm.m 1.00 ohm.m 1.04 ohm.m 1.08 ohm.m 1.12 ohm.m 1.15 ohm.m 1.17 ohm.m 11.8 W/m.C 13.5 W/m.C 15.4 W/m.C 17.1 W/m.C 18.6 W/m.C 20.5 W/m.C 22.4 W/m.C 11.6 m/m.C 12.0 m/m.C 12.4 m/m.C 12.7 m/m.C 13.1 m/m.C 13.3 m/m.C 0.0334 cm/s 0.0362 cm/s 0.0398 cm/s 0.0427 cm/s 0.0454 cm/s 0.0489 cm/s 0.0517 cm/s 412 J/kg.C 434 J/kg.C 451 J/kg.C 465 J/kg.C 477 J/kg.C 488 J/kg.C 504 J/kg.C 223 GPa 218 GPa 211 GPa 209 GPa 205 GPa 195 GPa 181 GPa 1304 - 1368C British Units RT 0.311 lb/in. RT 0.312 lb/in. RT 38.4 ohm.in 200F 39.3 ohm.in 400F 41.1 ohm.in 600F 42.8 ohm.in 800F 44.3 ohm.in 1000F 45.5 ohm.in 1100F 46.0 ohm.in RT 82 btu.in/h.ft.F 200F 93 btu.in/h.ft.F 400F 107 btu.in/h.ft.F 600F 120 btu.in/h.ft.F 800F 132 btu.in/h.ft.F 1000F 147 btu.in/h.ft.F 1100F 154 btu.in/h.ft.F 70-200F 6.4 in/in.F 70-400F 6.7 in/in.F 70-600F 6.9 in/in.F 70-800F 7.1 in/in.F 70-1000F 7.3 in/in.F 77-1100F 7.4 in/in.F RT 0.129 ft/h 200F 0.139 ft/h 400F 0.155 ft/h 600F 0.167 ft/h 800F 0.180 ft/h 1000F 0.194 ft/h 1100F 0.200 ft/h RT 0.098 btu/lb.F 200F 0.103 btu/lb.F 400F 0.108 btu/lb.F 600F 0.112 btu/lb.F 800F 0.115 btu/lb.F 1000F 0.118 btu/lb.F 1100F 0.120 btu/lb.F RT 32.3 x 106 psi 200F 31.6 x 106 psi 400F 30.5 x 106 psi 600F 30.2 x 106 psi 800F 29.5 x 106 psi 1000F 27.6 x 106 psi 1100F 26.4 x 106 psi 2380 - 2495F
Thermal Conductivity
Thermal Diffusivity
Specific Heat
Melting Range
* Properties are for material in the age-hardened condition unless otherwise noted. HAYNES C-22HS alloy
Alloy 316L 725 (age hardened) 625 C-276 C-22HS (age-hardened) C-22 C-22HS (mill annealed)
Critical Pitting Temperature C F 15 59 85 185 100 212 >120 >248 110 230 >120 >248 >120 >248
Alloy 316L 725 (age hardened) 625 C-276 C-22HS (age-hardened) C-22 C-22HS (mill annealed)
Critical Pitting Temperature C F 25 77 75 167 90 194 105 221 110 230 120 248 >130 >266
Duration
30 days
Environment Deaerated 20% NaCl, 508 psig CO2, 508 psig H2S Deaerated 25% NaCl, 508 psig CO2, 508 psig H2S
RATIO RATIO RATIO Time(env) Elong.(env) R.A.(env) Time(inert) Elong.(inert) R.A.(inert) 0.98 0.98 0.87 0.97 0.97 0.83
Hydrochloric Acid
Hydrobromic Acid
Hydrofluoric Acid
Sulfuric Acid
Nitric Acid
Phosphoric Acid
C-22 mm/y mpy 0.06 2.2 1.44 56.6 0.01 0.4 0.20 7.7 0.02 0.6 0.01 0.3 0.45 17.8 0.01 0.3 0.46 18.2 0.21 8.2 0.15 6.0 0.33 13.1 0.53 21.0 0.04 1.6 0.28 11.0 0.68 26.8 0.31 12.3 0.40 15.9 N/T* N/T 0.28 11.0 N/T N/T 0.34 13.3 0.06 2.3 0.03 1.2 0.08 3.0 0.03 1.3 0.56 21.9 1.04 41.0 3.02 119.0 0.13 5.0 1.02 40.0 0.20 8.0
*N/T = not tested **G 28A = 50% H2SO4 + 42 g/l Fe2(SO4)3 ***G 28B = 23% H2SO4 + 1.2% HCl + 1% FeCl3 + 1% CuCl2 HAYNES C-22HS alloy 6
Hydrochloric Acid
Hydrobromic Acid
Hydrofluoric Acid
Sulfuric Acid
Nitric Acid
Phosphoric Acid
*N/T = not tested **G 28A = 50% H2SO4 + 42 g/l Fe2(SO4)3 ***G 28B = 23% H2SO4 + 1.2% HCl + 1% FeCl3 + 1% CuCl2 7
ISO-CORROSION DIAGRAMS
Each of these iso-corrosion diagrams was constructed using numerous corrosion rate values, generated at different acid concentrations and temperatures. The blue line represents those combinations of hydrochloric acid concentration and temperature at which a corrosion rate of 0.1 mm/y (4 mils per year) is expected, based on laboratory tests. Below the line, rates under 0.1 mm/y are expected. Similarly, the red line indicates the combinations of acid concentration and temperature at which a corrosion rate of 0.5 mm/y (20 mils per year) is expected. Above the red line, rates of over 0.5 mm/y are expected. Between the blue and red lines, corrosion rates are expected to fall between 0.1 and 0.5 mm/y. Annealed
ISOCORROSION DIAGRAMS
Age-Hardened
MECHANICAL PROPERTIES
Typical Tensile Data for Cold-Rolled and Solution Annealed Sheet
Metric Units Temperature C RT 100 200 300 400 500 600 0.2% Offset Yield Strength MPa 439 394 343 316 308 296 288 Ultimate Tensile Strength MPa 837 807 754 734 718 691 665 Elongation % 57.3 59.9 58.6 66.8 69.6 67.8 69.9 Temperature F RT 200 400 600 800 1000 1200 British Units 0.2% Offset Yield Strength ksi 63.6 57.6 49.4 45.3 44.4 42.2 40.1 Ultimate Tensile Strength ksi 121.4 117.4 108.9 106.0 103.6 98.3 94.8 Elongation % 57.3 60.0 58.5 68.2 70.1 66.5 68.5
Typical Tensile Data for Hot-Rolled and Solution Annealed Plate and Bar
Metric Units Temperature C RT 100 200 300 400 500 600 0.2% Offset Yield Strength MPa 376 329 288 263 255 241 223 Ultimate Reduction Tensile Elongation Temperature in Area Strength MPa 806 767 721 695 677 652 628 % 62.3 66.7 65.9 68.8 69.5 69.3 70.6 % 77.5 78.0 77.3 75.2 73.0 70.9 69.1 F RT 200 400 600 800 1000 1200 British Units 0.2% Offset Yield Strength ksi 54.4 48.0 41.4 37.5 36.7 34.1 31.3 Ultimate Reduction Tensile Elongation in Area Strength ksi 117.0 111.7 104.2 100.2 97.5 93.0 90.1 % 62.3 66.8 65.8 69.2 69.6 69.1 71.4 % 77.5 78.6 77.1 74.9 72.3 70.2 67.7
10
MECHANICAL PROPERTIES
Typical Tensile Data for Cold-Rolled, Solution Annealed, and Age-Hardened Sheet
Metric Units Temperature C RT 100 200 300 400 500 600 0.2% O ffset Yield Strength MPa 759 710 658 630 590 572 547 Ultimate Tensile Strength MPa 1230 1190 1131 1103 1049 1003 928 Elongation Temperature % 40.9 43.6 43.4 47.8 48.2 47.1 46.3 F RT 200 400 600 800 10 00 11 00 British Units 0.2% O ffset Yield Strength ksi 110.0 103.5 95.0 90.7 84.1 82.3 79.8 Ultimate Ten sile Strength ksi 178.4 173.1 163.6 159.5 149.8 143.3 135.2 Elongation % 40.9 43.7 43.3 48.5 48.1 46.6 46.4
Typical Tensile Data for Hot-Rolled, Solution Annealed, and Age-Hardened Plate and Bar
Metric Units 0.2% Offset Temperature Yield Strength C MPa RT 690 100 627 200 579 300 539 400 518 500 507 600 488 0.2% Ultimate Reduction Offset Tensile Elongation Temperature in Area Yield Strength Strength MPa % % F ksi 1202 44.2 57.7 RT 100.1 1153 47.7 55.7 200 91.3 1089 48.3 60.0 400 83.7 1047 52.7 63.9 600 77.3 1006 52.3 63.4 800 74.3 964 50.3 63.2 1000 73.1 902 49.2 66.9 1100 70.9 British Units Ultimate Reduction Tensile Elongation in Area Strength ksi 174.2 167.9 157.5 150.9 144.4 137.4 131.5 % 44.2 47.7 48.3 53.3 52.3 49.3 49.0 % 57.7 55.5 60.2 64.5 63.0 63.2 66.5
Test Temperature F C -320 -196 Room Room -320 -196 Room Room
Average Charpy V-Notch Impact Energy ft.-lbs. Joules 226 306 > 260 > 353 73 99 112 151
11
THERMAL STABILITY
HASTELLOY C-22HS alloy has excellent retained ductility and impact strength after long term thermal exposure at elevated temperatures. The data below shows the tensile and impact properties of samples machined from plate following long term thermal exposure at 800 and 1100F (427 and 593C).
Original Condition Annealed Annealed Annealed Annealed Annealed Annealed Annealed Age-Hardened Age-Hardened Age-Hardened Age-Hardened Age-Hardened Age-Hardened Age-Hardened
Exposure Temp. F --800 800 800 1100 1100 1100 --800 800 800 1100 1100 1100 C --427 427 427 593 593 593 --427 427 427 593 593 593
12
465
67.5
791
114.7
44
759
110.1
1101
159.7
23
458
66.4
708
102.7
39.2
735
106.6
1062
154.1
28.9
442
64.1
785
113.9
46.2
758
110.0
1129
163.7
27.5
434
62.9
780
113.1
39.4
763
110.6
1120
162.5
17.8
455
66.0
724
105.0
53.1
712
103.3
1054
152.9
36.8
13
Fabrication Heat Treatment Wrought forms of C-22HS alloy are furnished in the solution annealed condition, unless otherwise specified. The standard solution annealing treatment consists of heating to 1975F (1080C) followed by rapid air-cooling or water quenching. Parts which have been hot formed should be solution annealed prior to final fabrication or installation. To use the alloy in the high-strength condition, it is necessary to age-harden using a two step treatment of 1300F (705C) for 16 hours, furnace cooling to 1125F (605C) and holding at that temperature for 32 hours, followed by an air cool. Cold or hot-worked structures should normally be given a full solution anneal prior to performing the age-hardening treatment. Forming C-22HS alloy has excellent forming characteristics, and cold forming is the preferred method of shaping. The alloy can be easily cold worked due to its good ductility. The alloy is generally stiffer than the austenitic stainless steels; therefore more energy is required during cold forming. For further information on the fabrication of C-type alloys, please consult publication H-2010. Machining C-22HS alloy may be machined in either the solution annealed or age-hardened condition. Carbide or ceramic tools are recommended. For use in the age-hardened condition, it is suggested to rough machine in the annealed condition. After performing the age-hardening heat treatment, light machining may be performed to achieve desired final dimensions.
14
Health and Safety Welding can be a safe occupation. Those in the welding industry, however, should be aware of the potential hazards associated with welding fumes, gases, radiation, electric shock, heat, eye injuries, burns, etc. Also, local, municipal, state, and federal regulations (such as those issued by OSHA) relative to welding and cutting processes should be considered. Nickel-, cobalt-, and iron-base alloy products may contain, in varying concentrations, the following elemental constituents: aluminum, cobalt, chromium, copper, iron, manganese, molybdenum, nickel and tungsten. For specific concentrations of these and other elements present, refer to the Material Safety Data Sheets (MSDS) available from Haynes International, Inc. Inhalation of metal dust or fumes generated from welding, cutting, grinding, melting, or dross handling of these alloys may cause adverse health effects such as reduced lung function, nasal and mucous membrane irritation. Exposure to dust or fumes which may be generated in working with these alloys may also cause eye irritation, skin rash and effects on other organ systems The operation and maintenance of welding and cutting equipment should conform to the provision of American National Standard ANSI/AWS Z49.1, "Safety in Welding and Cutting". Attention is especially called to Section 4 (Protection of Personnel) and 5 (Health Protection and Ventilation) of ANSI/AWS Z49.1. Mechanical ventilation is advisable and, under certain conditions such as a very confined space, is necessary during welding or cutting operations, or both, to prevent possible exposure to hazardous fumes, gases, or dust that may occur.
15
STANDARD PRODUCTS
By Brand or Alloy Designation: HASTELLOY Family of Corrosion-Resistant Alloys
HAYNES International
B-3, C-4, C-22, C-276, C-2000 , C-22HS, G-30, G-35, G-50, HYBRID-BC1, and N
Wear-Resistant Alloy
6B
Standard Forms: Bar, Billet, Plate, Sheet, Strip, Coils, Seamless or Welded Pipe & Tubing,
Pipe Fittings, Flanges, Fittings, Welding Wire, and Coated Electrodes
Properties Data: The data and information in this publication are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature, and are believed to be reliable. However, Haynes does not make any warranty or assume any legal liability or responsibility for its accuracy, completeness, or usefulness, nor does Haynes represent that its use would not infringe upon private rights.
Any suggestions as to uses and applications for specific alloys are opinions only and Haynes International, Inc. makes no warranty of results to be obtained in any particular situation. For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Material Safety Data Sheet supplied by Haynes International, Inc. All trademarks are owned by Haynes International, Inc.
Global Headquarters
1020 West Park Avenue P.O. Box 9013 Kokomo, Indiana 46904-9013 (USA) Phone: 1-800-354-0806 or (765) 456-6012 Fax: (765) 456-6905
www.haynesintl.com