2-Shot Overmolding Thermoplastics / Elastollan TPU Without Plasma - Treatment
2-Shot Overmolding Thermoplastics / Elastollan TPU Without Plasma - Treatment
2-Shot Overmolding Thermoplastics / Elastollan TPU Without Plasma - Treatment
Elastollan
PA 6
good bonding
PC, PC / ABS
good bonding
good bonding
PA 6.6, PA 12
poor bonding
PBT
poor bonding
PE, PP, PS
no bonding
POM
no bonding
TPU / no Plasma
PA 6
good bonding
perfect bonding
PC, PC / ABS
good bonding
perfect bonding
good bonding
perfect bonding
PA 6.6, PA 12
poor bonding
good bonding
PBT
poor bonding
perfect bonding
PE, PP, PS
no bonding
good bonding
POM
no bonding
poor bonding
Thermoplastic
ABS
ABS/PC
PA 6
PA 6 25GF
PA 6.6
PA 6.6 25GF
PBT
PC
PS
SAN
PP
TPU
(Elastollan)
Description
P Plasmatreated (excellent Bonding)
no P
P
P
P
P
P
excellent Bonding
good Bonding
Bonding
light Bonding
no Bonding
no P
P
P
P
S EB S
TPE
TPU
P P/E PDM
EPDM
Elastome rs
NR
SB R
ABS
PA 6
P A 66
P A 6 12
PBT
PC
P MMA
P OM
PP
m PPE
SAN
Good Bonding
Poor Bonding
No Bonding
LS R
1180A
7
5
7
8
N.G.
7
8
4
7
8
7
7
N.G.
7
5
8
9
1185A
6
8
8
9
N.G.
9
11
C85A
8
4
8
7
N.G.
8
9
S85A
7
8
6
9
N.G.
8
14
9
10
8
8
N.G.
7
5
C78A
9
6
8
8
N.G.
8
9
3
8
7
7
6
N.G.
9
6
6
7
6
6
N.G.
5
4
9
6
7
8
8
9
7
SP876
9
5
8
10
N.G.
10
10
3
7
8
8
8
6
10
N.B.
N.B.
12
10
Units = N/mm
N.B. = No Break
N.G. = No Grip/No Bond
Reference Test Method - Iso 527-2/1A, 200 mm/min (Tensile Test)
1180A
5
4
6
5
7
4
6
6
5
4
7
N.G.
6
8
1185A
9
5
5
9
N.G.
6
6
N.G.
6
4
4
N.G.
4
N.G.
11
C78A
3
5
4
8
N.G.
6
4
3
N.G.
5
4
4
N.G.
10
N.G.
3
8
Units = N/mm
N.B. = No Break
N.G. = No Grip/No Bond
Reference Test Method - Iso 527-2/1A, 200 mm/min (Tensile Test)
C85A
S85A
6
7
6
7
N.G.
6
6
N.G.
N.G.
5
N.G.
N.G.
N.G.
8
N.G.
SP876
10
7
5
8
N.G.
9
6
3
N.G.
7
5
6
N.G.
6
N.G.